The International Journal Of Engineering And Science (IJES)
||Volume|| 2 ||Issue|| 11 ||Pages|| 18-24 ||2013||
ISSN (e): 2319 – 1813 ISSN (p): 2319 – 1805

Corrosion Properties of Plain Carbon Steels
Engr Dr A.C Uzorh
Head of Department, Mechanical Engineering Department
Federal University of Technoloy Owerri PMB 1526 Owerri, Imo State, Nigeria.
----------------------------------------------------------ABSTRACT----------------------------------------------------------This paper looks at the corrosion characteristics of two grades of plain carbon steels of Ajaokuta steel company
limited, namely, DIN 35-2 (Ribbed rod) and DIN 37-2 (plain rod). In three environments: Salt solution, Tap
water and Moist soil. The company is located in Northern Nigeria. The corrosion characteristics of these two
grades of plain carbon steel were studied under cold work condition and as rolled or untreated condition in the
aforementioned media for a period of 22 days. Result obtained show that corrosion rates increases with
increasing degree of cold work. In addition, it was found that corrosion rates of these products vary in the
different corroding media with moist soil having the highest corrosive ability, followed by tap water and then
3% by weight of sodium chloride salt solution. Also the rib rod samples essentially corroded more than the
plain rod samples in these various environments.

Keywords: Corrosion, Plain Carbon Steels, Cold work,
------------------------------------------------------------------------------------------------------------ ---------------------------Date of Submission: 11 March, 2013
Date of Acceptance: 10, November 2013
-------------------------------------------------------------------------------------------------------- --------------------------------

I. INTRODUCTION
Corrosion is recognized as a major problem both in developed and developing nations of the world.
Millions of naira are being spent every year to control tosses of corrosion. With the added interest of steel
technology and steel production in Nigeria, it is of paramount importace that thorough studies and investigations
be carried out to estimate how these steel products behave in use. In this respect, their corrosion properties are of
paramount importance.
This paper looks at the corrosion properties of steels produced by Ajaokuta Steel company limited in
different corroding environments namely: tap water, moist soil and 3% by weight of sodium chloride solution.
Three percent of sodium chloride was used because its corrosive ability had been studied and known. Also salt
solution stimulates the natural sea water in the laboratory because sea water in the laboratory does not truly
represent the natural environment. This is also a consequence of the changes that occur in it on storage. Majorly
the research will dwell on the two common known steels:
1)
2)

Plain carbon steel
Alloy steels (UHLIG+, H.H. 1963)

Experiment is carried out on plain carbon steel because they are the most common sued steels in the industries.
Plain carbon steels are divided into three groups:
1)
2)
3)

low carbon steel
medium carbon steel
high carbon steels

Steel – Carbon Steel
It is an alloy of iron and carbon, with carbon content up to maximum of 1.5 – 2.0%. The carbon occurs
in the form of iron carbide, because of its ability to increase the hardness and strength of the steel. Other certain
elements like silicon, phosphorus, sulphur and manganese are also present in greater or lesser amount to impart
certain amount of desirable properties to it. Most of the steels produced recently is the plain carbon steel or
carbon steel. A carbon steel is defined as a steel which has its properties mainly due to its carbon content and
does not contain more than 0.5% of silicon and 1.5% of manganese. (R.S Khurmi, J.K. Gupta 2005)
(DEUTCHMAN, A.D. et al 1975). The plain steels are usually classified in their carbon content, the commonest
of the range being mild steel carbon content. (W.A.J. Champion 1972).

www.theijes.com

The IJES

Page 18
Corrosion Properties of Plain Carbon Steels...
APPLICATIONS OF CARBON STEELS (Chapman 1985)
CARBON %
Dead mild 0.1-0.125
Mild (low) 0.15-0.3
0.3-0.5 (0.05% - 0.30)
Medium carbon (0.5 – 0.7)
0.7 – 0.9 (0.3% - 0.5%)
High carbon (0.9-1.1)
1.1 – 1.4 (0.50% - 2.0%)

USES
Wire rod, thin sheets, solid drawn tubes, etc
Boiler plates, bridge work, structural sections, drop
forgings, general workshop purposes.
Axes, drop forging, high tensile tubes and wire
agricultural tools.
Springs, locomotive tyres, large forging dies, wire
ropes, hammers and snaps for riveters.
Springs, small forging dies, spear blades, cold setts,
wood chisels.
Cold chisels, press dies, punches, secrewing dies, wood
working tools axes, picks.
Razors, hand files, drills,gauges, metal-cutting tools.

This research paper is expected to help us understand how steel products of Ajaokuta Steel company
and other related steel products corrode in different environments. It will also assist in finding means of
minimizing or even preventing corrosion for it is said that “an ounce of prevention is worth a pound a pound of
cure”. Or better say “prevention is better than cure”.
Plain Carbon Steel
The two types of carbon steels are plain carbon steel and alloy steel. Plain carbon steel is one which
contains in addition to carbon and iron certain elements notably manganese, phosphorus, supphur and silicon in
small quantities. It may also contain traces of elements like: copper, boron, cobalt and so on.
Plain carbon steel is divided into three groups:
1)
low carbon steel
2)
medium carbon steel
3)
high carbon steel
(YOUNG, J.F.1982 Materials and Processes).
Hot And Cold Working Of Plain Carbon Steel
Rolling , forging, drawing, compression and extrusion and typical methods by which metals are
worked especially steels have great effects on their mechanical and metallurgical properties. Cold working
refers to the act of permanently deforming a cold metal. The term cold is relative. Even room temperature may
be hot for such metals i.e as lead. A metal is said to be cold when it is worked at a temperature below
recrystallization temperature but below the melting or boiling point is termed hot working. Metals are subjected
to mechanical working for two general purposes:
a)

To reduce the original block or slug of metal approximately to the finished dimension of the part or mill
form, thereby saving material, machining cost and time.
b) To improve the mechanical properties of the material thoroughly
Definition of Corrosion
Corrosion may be defined broadly as the destruction or deterioration of metal by direct chemical and
electro-chemical reaction with its environment. Most simply stated, metallic corrosion is the reverse of
electroplating. The metal being corroded forms the anode while the cathode is that being electroplated. Metallic
corrosion occurs because in many environment most metals are not inherently stable and tend to revert to some
more stable combination of which the metallic ores as found in nature are familiar examples.
Factors Influencing Corrosion Of Plain Carbon Steels
Generally, the factors affecting the rate of corrosion of plain carbon steels are either material dependent
or environment-dependent or a combination of both . Some of the factors which are associated mainly with
metals are:
1) Over voltage of metal on the hydrogen.
2) Chemical and physical homogeneity of the metal surface.
3) Inherent ability to form an insoluble protective film
4) Hydrogen ion Activity (PH) in the solution
5) Influence of oxygen in the solution adjancent to the metal
6) Rate of flow of solution in contact with metal

www.theijes.com

The IJES

Page 19
Corrosion Properties of Plain Carbon Steels...
Significance of Corrosion
Corrosion has a lot of significance economically, socially and otherwise. This led J.M. West to write,
"Corrosion kills people, waste resources and cost money we can ill afford". But except for a few corrosion
reactions which are of practical importance for example, the corrosion of metallic lead, the effects of corrosion
are nothing to write home about.
Some of the disadvantage of corrosion includes:
(a)
(b)
(c)
(d)

Wastage of material, money, time and man power due to over design, because of corrosion.
Contamination of products eg damage of entire batch of soap by a corroded copper
Cost of replacing corroded structure or components
Loss of products for example oil or gas losses in corroded pipes.

II.

METHODOLOGY

In this chapter, the focus includes methods and techniques adopted as well as the materials used for this
study. This contains material used, working samples adopted and relevant carbon test carried out.

III.

DESCRIPTION

Ajaokuta steel company limited was visited and some relevant materials were obtained for the study
from this company. The material gotten from the company is Plain Carbon steel in the form of 16mm plain
rolled rods ( steel grade: DIN 37-2) and 16mm ribbed rods (DIN 35-2). These rods were subsequently reduced
to the required dimensions for the experiment using the lathe machine, grinding machine and hack saw. The
diagram below shows reduction procedure adopted using the lathe machine.
Mounting steel/rod on a lathe machine for reduction process

Fig 3.2: Reduction process of steel/rod on a Lathe Machine

After machining the materials they were further polished and cleaned with emery paper.The ribbed
rods were reduced to 10mm in diameter and 20mm by length, this was done to ensure that ribs were completely
removed for easier calculation of the exposed surface areas of the specimens. Then the plain rolled rods were
reduced to 13mm in diameter and 20mm in length. All these measurements were done using the vernier callipers.
These diameters were chosen in this manner wit diameter of samples being about one-half the length, to enable
us compress the sample without them experiencing buckling effects. Specimens produced were 108: 56 plain
rolled rod and 56 ribbed rod.

www.theijes.com

The IJES

Page 20
Corrosion Properties of Plain Carbon Steels...
Cold Working Of Samples
Coldworking of samples was achieved by compression. The compressive behaviours of each of the two
different materials was determined using the 40-ion universal testing machine (UTM) in the laboratory. The
testing was done to determine the different degrees of compression to which the material could be subjected
without necessarily crushing them.
18 specimens of the ribbed rod were subjected to a compressive load of 7000kgf which compressed the
length from 20mm to 17.8mm and enlarged the diameter from 10mm to 10.6mm. Also 18 more specimens of
the ribbed rod were subjected to a compressive load of 7500kfg reducing the length of each of the 18 specimens
from 20mm to approximately 15.7mm with diameter enlarged to 11.29mm. The percentage of cold work in the
above two cases were calculated as follows:
% cold work (%CW) = Change in cross-sectional area
Original corss-sectional area
%CW : 1 = 12.36%
%CW : 2 = 27.5%
Similarly, 18 plain rolled samples were given about 16% cold work by subjecting them to a
compressive load of 7500kgf which compressed each of them from a length of 26mm to 22.4mm and increased
their diameter approximately from 13mm to 1.401mm. In addition, 18 more samples of plain rolled rod were
subjected to 9000kgf(compressive load) which gave about 30% cold work to each of them by reducing their
length from 13mm to 1.482mm.
Corrosion Tests
Preparation Of Corroding Media
Three types of corroding media were used, namely
1) Tap water – a sufficient quantity of weight 890 per bowl was used. The quantity was large enough for
complete immersion of the corrosion specimen.
2) Moist soil – sandy loam soil of the following properties was used: PH value in H20=4.2, in Kcl=3.7
3) NACL solution – 3% by weight of NACL solution was used. The solution coomprised of distilled water and
common salt(NaCl), mass of distilled water used per bowl was 790g. using the electronic weighing balance,
mass of NaCl was 24.432g
Corrosion Of Samples
Eighteen plastic bowls were provied for eighteen groups of sample products. Specimens were weighed
with electronic weighing balance, wih exposed surface area calculated. The compressed samples were again
measured to determine the changes in lengths with new diameters calculated. The samples were arranged in
three subscripts i.e tap water, salt solution and moist soil respectively. Care was taken not to allow samples to
touch one another in order not to initiate galvanic action. As corrosion of samples proceeded day after day,
distilled water was added to the salt solution or tap water solution to make up for losses due to evaporation.
Decrease in the moisture conent was noticed by occasionally filling and reweighing the bowls to determine the
loss in weight.
Determination of Weight Lost
No corrosion of sample was noticed the first day, corrosion was noticed the third day and care was
taken to remove only the corrosion products. The samples were weighed with electronic weighing balance to
determine their new weights. The weight loss of each of the samples was determined and recorded. The process
of washing,drying,weighing,deterination of weight loss and recording was repeated for the 6 th, 10th, 14th, 18th,
22nd days.
Experimental Results And Analysis
The lengths, diameter and surface areas for the three groups of each of the two grades of plain carbon
steel namely DIN 35-2(ribbed rod) and DIN37-2(plain rod) are given in the tables of three samples ( As Rolled
Samples ARS; Compressed Samples with 1st degree of cold work CDW1 and Compressed samples with second
degree of cold work CDW2) below:

www.theijes.com

The IJES

Page 21
Corrosion Properties of Plain Carbon Steels...
Table 4.1 TYPICAL INITIAL PARAMETERS for Ribbed Rod (Din 35-2) Samples
Group
ARS
CDW1
CDW2

Diameter,D (cm)
1.000
1.060
1.129

Length,L (cm)
2.00
1.78
1.57

Total Surface Area(cm2)
7.8540
7.6925
7.5708

Table 4.2 TYPICAL INITIAL PARAMETERS for Plain Rod (DIN37-2) Samples
Group
ARS
CDW1
CDW2

Diameter,D (cm)
1.300
1.400
1.482

Length,L (cm)
2.60
2.24
2.00

Table 4.3 As Rolled Samples(ARS), Group 1
DAYS

SAMPLES

0
3
6
10
14
18
22

A
B
C
D
E
F
G

Material: Ribbed Rod

INITIAL
WEIGHT
(kg)
12.110
12.115
11.987
12.105
12.082
11.985
12.110

WEIGHT LOSS
(mg)
0
4
13
24
32
37
53

Table 4.4 Compressed Samples (CDW1), Group 2
DAYS

SAMPLES

0
3
6
10
14
18
22

H
I
J
K
L
M
N

INITIAL
WEIGHT
(kg)
12.154
11.943
12.148
12.001
12.110
12.010
12.154

0
12
19
28
37
48
57

SAMPLES

0
3
6
10
14
18
22

O
P
Q
R
S
T
U

INITIAL
WEIGHT
(kg)
12.000
11.997
12.090
12.011
11.989
12.003
12.000

Table 4.6 As Rolled Samples(ARS), Group 4
DAYS

SAMPLES

0
3
6
10
14
18
22

A2
B2
C2
D2
E2
F2
G2

www.theijes.com

INITIAL
WEIGHT
(kg)
12.103
12.002
12.000
11.998
12.100
11.993
12.103

WEIGHT LOSS
(mg)
0
13
22
32
41
50
60

0
3
9
18
28
33
37

The IJES

WEIGHT
LOSS/SURFACE
AREA(mg/cm2)
0.0000
0.5093
1.6552
3.0558
4.0743
4.7109
6.7482

Medium: Tapwater

EXPOSED
SURFACE
AREA(CM2)
7.6925
7.6925
7.6925
7.6925
7.6925
7.6925
7.6925

WEIGHT
LOSS/SURFACE
AREA(mg/cm2)
0.0000
1.5600
2.4699
3.6399
4.8271
6.2398
7.4098

Material: Ribbed Rod
EXPOSED
SURFACE
AREA(CM2)
7.5708
7. 5708
7. 5708
7. 5708
7. 5708
7. 5708
7. 5708

Material: Ribbed Rod
WEIGHT LOSS
(mg)

Medium: Tap Water

EXPOSED
SURFACE
AREA(CM2)
7.854
7.854
7.854
7.854
7.854
7.854
7.854

Material: Ribbed Rod
WEIGHT LOSS
(mg)

Table 4.5 Further Compressed Samples (CDW2), Group 3
Tapwater
DAYS

Total Surface Area(cm2)
13.2732
12.9422
12.7617

Medium:

WEIGHT
LOSS/SURFACE
AREA(mg/cm2)
0.0000
1.7171
2.9059
4.2267
5.4155
6.6043
7.9252

Medium: NaCl Solution

EXPOSED
SURFACE
AREA(CM2)
7.854
7.854
7.854
7.854
7.854
7.854
7.854

WEIGHT
LOSS/SURFACE
AREA(mg/cm2)
0.0000
0.3819
1.1459
2.2918
3.5651
4.2017
4.7110

Page 22
Corrosion Properties of Plain Carbon Steels...
Table 4.7 Compressed Samples (CDW1), Group 5
DAYS

SAMPLES

0
3
6
10
14
18
22

H2
I2
J2
K2
L2
M2
N2

Table 4.8
DAYS

0
3
6
10
14
18
22

INITIAL
WEIGHT
(kg)
12.101
12.237
11.990
11.989
12.001
12.121
12.101

Material: Ribbed Rod
WEIGHT LOSS
(mg)
0
7
10
19
29
38
43

Medium: NaCl Solution

EXPOSED
SURFACE
AREA(CM2)
7.6925
7.6925
7.6925
7.6925
7.6925
7.6925
7.6925

WEIGHT
LOSS/SURFACE
AREA(mg/cm2)
0.0000
0.0100
1.3000
2.4699
3.7699
4.9399
5.5899

Further Compressed Samples (CDW2), Group 6 Material: Ribbed Rod
Medium: NaCl Solution
SAMPLES
INITIAL
WEIGHT LOSS EXPOSED
WEIGHT
WEIGHT
(mg)
SURFACE
LOSS/SURFACE
(kg)
AREA(CM2)
AREA(mg/cm2)
O2
12.172
0
7.5708
0.0000
P2
11.987
8
7. 5708
1.0567
Q2
11.998
13
7. 5708
1.7171
R2
12.003
21
7. 5708
2.7738
S2
11.997
31
7. 5708
4.0947
T2
12.013
40
7. 5708
5.2835
U2
12.172
46
7. 5708
6.0760

IV. OBSERVATION
After the first day, each samples were surrounded by yellowish deposits evident in the tap water than
salt solution. As days progress the deposits turned brown identified to be ferric hydroxide. Some shiny white
patches of particles were suspected to be ferrous hydroxide formed due to the presence of insufficient oxygen.
On withdrawal of specimed immersed in the moist soil, dark brown deposits of ferric hydroxide were noticed on
them.
The corroding media (tap water and salt solution) were observed to decrease continuously in volume
due to evaporation of water. The decrease in the volume of media was evident from the ringed marks on the
bowl inducating the original levels of the media. On washing of sample from salt solution and tap water, it was
observed that the deposit on them were relatively easily removed except for the dark patches of samples which
took quite some time, but samples of moist soil were not easily washed off.
Analysis Of Result
Based on the results deduced from the table, the analysis of result shows that on the whole, the ARS
have the lowest corrosion rate, followed by CDW1 and the CDW2 having the highest corrosion rate. If a graph
is plotted , the as rolled samples curve (ARS) will follow a gradual increase in corrosion attack on the first 6
days and then increase suddenly 4 days after followed by a gradual increase in the next 8 days and another
increase in the last 4 days. Curves CDW1 and CDW2, has relatively high corrosion on the first 6 days. On the
whole, the as rolled samples have the lowest corrosion rate , followed by CDW1 and with the CDW2 having the
highest corrosion rate. Sudden change in the rate of corrosion attacks of the metals mentioned could be
associated with the physical breakdown of the barrier films of the corrosion products which encourages
corrosion attacks by exposing new surface area of the metals.
In the case of moist soils the changes could be explained by the effect of making up of moisture loss
which tends to promote corrosion. The marked low corrosion rates in the initial days mentioned especially for as
rolled samples might be attributed to the effect of the surface finish of the samples. The as rolled samples have
better surface finish of the samples. The as rolled samples have etter surface finish than the compressed samples.
On the other hand the low corrosion rates experienced as the corrosion progressed after many days are likely
indications that the protective films (corrosion products) accumulated over the past days tend to lower the rates
of corrosion attack by not allowing enough contact between samples and corroding media.

www.theijes.com

The IJES

Page 23
Corrosion Properties of Plain Carbon Steels...
The general trend obtained whereby the compressed samples corroded higher than their corresponding
as rolled samples might be as a result of the increased rate of dissolution of the higher energy (strained) grains
produced by the cold work effect by the corroding media. The fact that the samples coldworked to a higher
degree corroded more than that cold worked to a lesser degree indicated that the increased rate of dissolution of
the high energy (strained) grains is highest for them.

V. CONCLUSION
In general, the rate of corrosion of plain carbon steels is dependent on both the environmental
conditions, structural and compositional properties of the steel. Within the limits of experimental error,
conclusions drawn based on observations and result of the research are:
1) In corroding media for example, NaCl solution, tap water and moist soil , corrosion of plain carbon steel
depends on the amount of oxygen dissolved in the media.
2) Among the three corroding media used in the experiment, moist soil has the highest corrosive ability
followed by tap water and then NaCl solution.
3) The degree of cold water increases the corrosion of plain carbon steels of Ajaokuta steel company limited.
4) Plain carbon steels of Ajaokuta steel company limited as comparable to its counerparts from other places.
Suggestions For Future Work
a)
To eliminate or reduce errors in future investigations of corrosion properties of materials by weght lost
per unit area method, the following are sugested:
b)
The use of a better means of removing adherent corrosion products, say by the use of chemical means.
c)
An open building with the roof covered for better air circulation than the present laboratory should be
provided for the experiment to allow better free circulation of air and real atmospheric condition to play
their natural parts in corrosion process without rain necessarily disrupting the project set up.
d)
It is suggested that future researchers wishing to investigate
properties of materials formulate
mathematical relations existing between the extent of corrosio attack and time as well as investigation of
corrosion properties of other steel products of Ajaokuta steel company limited and other local steel
producing companies.
Limitations Of Experimental Results
The possible sources of errors are likely to be from:
1)
The instument used: such errors include errors due to low sensitivity of instruments, faulty instruments
etc
2)
The method of preparing the samples by machining , grinding and cleaning with energy paper may not
have ensured uniform surface finish and dimensions where necessary. Also in the compression process,
the stress developed in the process may not have been uniformly distriuted.
3)
The physical method of removing corrosion products can introduce errors, since the corrosion product
may not be properly and completely removed.
4)
The atmospheric condition that obtains in the laboratory may not compare favourably with that obtained
in a better open place. Hence free circulation of air and real atmospheric conditions may not be allowed
to play their natural part in the corrosion well enough.

REFERENCES
[1].
[2].
[3].
[4].
[5].
[6].
[7].
[8].
[9].

Chapman, F. A. (1985): Corrosion testing procedures 2nd Edition, Chapman and Hall Publishers, Incorporated, London.
Duetchman, A.D. et al (1975): Machine Design, Theory and Practice, Collier Macmillian Publishers, (Inc) London.
J.k Gupta. (2005) : 4th Edition, R.S. Khurmi Machine Design.
West J.M. (1980) Basic corrosion and oxidation, Ellis Hordward Publishers, Manchester.
Young, J.F. (1982): 2nd edition, John Wiley and Sons, New York.
http://www.emeraldinsight.com/products/journals/journals.htm?id=acmm
http://www.engineeringtoolbox.com/corrosion-d_986.html
http://en.wikipedia.org/wiki/Corrosion
http://www.corrosionprevention.org.uk/

www.theijes.com

The IJES

Page 24

Weitere ähnliche Inhalte

Was ist angesagt?

Steel & Iron
Steel & IronSteel & Iron
Steel & Irongngr0810
 
Effect of anions in seawater to corrosion attack on passive alloys
Effect of anions in seawater to corrosion attack on passive alloysEffect of anions in seawater to corrosion attack on passive alloys
Effect of anions in seawater to corrosion attack on passive alloyseSAT Journals
 
Effect of anions in seawater to corrosion attack on
Effect of anions in seawater to corrosion attack onEffect of anions in seawater to corrosion attack on
Effect of anions in seawater to corrosion attack oneSAT Publishing House
 
Machining challenges in stainless steel – a review
Machining challenges in stainless steel – a reviewMachining challenges in stainless steel – a review
Machining challenges in stainless steel – a reviewIJARIIT
 
Finite Element Modeling for Effect of Fire on Steel Frame
Finite Element Modeling for Effect of Fire on Steel FrameFinite Element Modeling for Effect of Fire on Steel Frame
Finite Element Modeling for Effect of Fire on Steel FrameIJERA Editor
 
Effect of alloying element
Effect of alloying elementEffect of alloying element
Effect of alloying elementPavan Narkhede
 
International Journal of Engineering and Science Invention (IJESI)
International Journal of Engineering and Science Invention (IJESI)International Journal of Engineering and Science Invention (IJESI)
International Journal of Engineering and Science Invention (IJESI)inventionjournals
 
How clean are your bearing steels
How clean are your bearing steelsHow clean are your bearing steels
How clean are your bearing steelsMike Lewis
 
Experimental study on corrosion of steel in soil medium
Experimental study on corrosion of steel in soil mediumExperimental study on corrosion of steel in soil medium
Experimental study on corrosion of steel in soil mediumeSAT Journals
 
Metallurgy--intro
Metallurgy--introMetallurgy--intro
Metallurgy--introMoiz Barry
 
classification of metals -MEC 1
classification of metals -MEC 1classification of metals -MEC 1
classification of metals -MEC 1K.G.S. PRASAD
 
Using Steel In Solar Racking and Mounting
Using Steel In Solar Racking and MountingUsing Steel In Solar Racking and Mounting
Using Steel In Solar Racking and MountingJMCSteelGroup
 
Material selection for nitrogen based fertilizers plants
Material selection for nitrogen based fertilizers plantsMaterial selection for nitrogen based fertilizers plants
Material selection for nitrogen based fertilizers plantsPrem Baboo
 
An assessment of the microstraft
An assessment of the microstraftAn assessment of the microstraft
An assessment of the microstraftAlexander Decker
 

Was ist angesagt? (20)

Steel & Iron
Steel & IronSteel & Iron
Steel & Iron
 
Iron
IronIron
Iron
 
Effect of anions in seawater to corrosion attack on passive alloys
Effect of anions in seawater to corrosion attack on passive alloysEffect of anions in seawater to corrosion attack on passive alloys
Effect of anions in seawater to corrosion attack on passive alloys
 
Effect of anions in seawater to corrosion attack on
Effect of anions in seawater to corrosion attack onEffect of anions in seawater to corrosion attack on
Effect of anions in seawater to corrosion attack on
 
Ferrous material
Ferrous materialFerrous material
Ferrous material
 
Machining challenges in stainless steel – a review
Machining challenges in stainless steel – a reviewMachining challenges in stainless steel – a review
Machining challenges in stainless steel – a review
 
Iron & Steel
Iron & SteelIron & Steel
Iron & Steel
 
Finite Element Modeling for Effect of Fire on Steel Frame
Finite Element Modeling for Effect of Fire on Steel FrameFinite Element Modeling for Effect of Fire on Steel Frame
Finite Element Modeling for Effect of Fire on Steel Frame
 
Stainless steel
Stainless steelStainless steel
Stainless steel
 
Classification of steel
Classification of steelClassification of steel
Classification of steel
 
Effect of alloying element
Effect of alloying elementEffect of alloying element
Effect of alloying element
 
International Journal of Engineering and Science Invention (IJESI)
International Journal of Engineering and Science Invention (IJESI)International Journal of Engineering and Science Invention (IJESI)
International Journal of Engineering and Science Invention (IJESI)
 
How clean are your bearing steels
How clean are your bearing steelsHow clean are your bearing steels
How clean are your bearing steels
 
Experimental study on corrosion of steel in soil medium
Experimental study on corrosion of steel in soil mediumExperimental study on corrosion of steel in soil medium
Experimental study on corrosion of steel in soil medium
 
Metallurgy--intro
Metallurgy--introMetallurgy--intro
Metallurgy--intro
 
classification of metals -MEC 1
classification of metals -MEC 1classification of metals -MEC 1
classification of metals -MEC 1
 
Using Steel In Solar Racking and Mounting
Using Steel In Solar Racking and MountingUsing Steel In Solar Racking and Mounting
Using Steel In Solar Racking and Mounting
 
American welding society dissimilar ferritic stainless steel
American welding society dissimilar ferritic stainless steelAmerican welding society dissimilar ferritic stainless steel
American welding society dissimilar ferritic stainless steel
 
Material selection for nitrogen based fertilizers plants
Material selection for nitrogen based fertilizers plantsMaterial selection for nitrogen based fertilizers plants
Material selection for nitrogen based fertilizers plants
 
An assessment of the microstraft
An assessment of the microstraftAn assessment of the microstraft
An assessment of the microstraft
 

Andere mochten auch

G021201054057
G021201054057G021201054057
G021201054057theijes
 
The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)theijes
 
A021201001014
A021201001014A021201001014
A021201001014theijes
 
I032030075081
I032030075081I032030075081
I032030075081theijes
 
The International Journal of Engineering and Science (The IJES)
 The International Journal of Engineering and Science (The IJES) The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)theijes
 
The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)theijes
 
The International Journal of Engineering and Science (The IJES)
 The International Journal of Engineering and Science (The IJES) The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)theijes
 
L03401071075
L03401071075L03401071075
L03401071075theijes
 
B02120307013
B02120307013B02120307013
B02120307013theijes
 
G03202048050
G03202048050G03202048050
G03202048050theijes
 
B03405012020
B03405012020B03405012020
B03405012020theijes
 
The International Journal of Engineering and Science (The IJES)
 The International Journal of Engineering and Science (The IJES) The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)theijes
 
I021203057060
I021203057060I021203057060
I021203057060theijes
 
The International Journal of Engineering and Science (IJES)
The International Journal of Engineering and Science (IJES)The International Journal of Engineering and Science (IJES)
The International Journal of Engineering and Science (IJES)theijes
 
D03202018036
D03202018036D03202018036
D03202018036theijes
 
B021201015023
B021201015023B021201015023
B021201015023theijes
 
A03240107
A03240107A03240107
A03240107theijes
 
B03202006011
B03202006011B03202006011
B03202006011theijes
 
G021203040047
G021203040047G021203040047
G021203040047theijes
 

Andere mochten auch (19)

G021201054057
G021201054057G021201054057
G021201054057
 
The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)
 
A021201001014
A021201001014A021201001014
A021201001014
 
I032030075081
I032030075081I032030075081
I032030075081
 
The International Journal of Engineering and Science (The IJES)
 The International Journal of Engineering and Science (The IJES) The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)
 
The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)
 
The International Journal of Engineering and Science (The IJES)
 The International Journal of Engineering and Science (The IJES) The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)
 
L03401071075
L03401071075L03401071075
L03401071075
 
B02120307013
B02120307013B02120307013
B02120307013
 
G03202048050
G03202048050G03202048050
G03202048050
 
B03405012020
B03405012020B03405012020
B03405012020
 
The International Journal of Engineering and Science (The IJES)
 The International Journal of Engineering and Science (The IJES) The International Journal of Engineering and Science (The IJES)
The International Journal of Engineering and Science (The IJES)
 
I021203057060
I021203057060I021203057060
I021203057060
 
The International Journal of Engineering and Science (IJES)
The International Journal of Engineering and Science (IJES)The International Journal of Engineering and Science (IJES)
The International Journal of Engineering and Science (IJES)
 
D03202018036
D03202018036D03202018036
D03202018036
 
B021201015023
B021201015023B021201015023
B021201015023
 
A03240107
A03240107A03240107
A03240107
 
B03202006011
B03202006011B03202006011
B03202006011
 
G021203040047
G021203040047G021203040047
G021203040047
 

Ähnlich wie The International Journal of Engineering and Science (The IJES)

Steel (construction material )
Steel (construction material )Steel (construction material )
Steel (construction material )Ali Rizgar
 
Comparative Study on the High-Stress Abrasive Wear Behaviour of Zinc and Copp...
Comparative Study on the High-Stress Abrasive Wear Behaviour of Zinc and Copp...Comparative Study on the High-Stress Abrasive Wear Behaviour of Zinc and Copp...
Comparative Study on the High-Stress Abrasive Wear Behaviour of Zinc and Copp...IRJET Journal
 
Studies on Corrosion Characteristics of Carbon Steel Exposed to Na2CO3, Na2SO...
Studies on Corrosion Characteristics of Carbon Steel Exposed to Na2CO3, Na2SO...Studies on Corrosion Characteristics of Carbon Steel Exposed to Na2CO3, Na2SO...
Studies on Corrosion Characteristics of Carbon Steel Exposed to Na2CO3, Na2SO...theijes
 
Heat treatment course material
Heat treatment course materialHeat treatment course material
Heat treatment course materialNeeraj Dhakar
 
Materialtechnologyforfertilizersindustries
MaterialtechnologyforfertilizersindustriesMaterialtechnologyforfertilizersindustries
MaterialtechnologyforfertilizersindustriesPrem Baboo
 
How we can use ECOrrosion positivelyin our life
How we can use ECOrrosion positivelyin our lifeHow we can use ECOrrosion positivelyin our life
How we can use ECOrrosion positivelyin our lifeAmrKhaled100
 
Corrosion assessment & recommendations
Corrosion assessment & recommendationsCorrosion assessment & recommendations
Corrosion assessment & recommendationsAbdul Hannan
 
X-RAY FLUORESCENCE BASED CHEMICAL COMPOSITION OF LADLE REFINERY FURNACE SLAG:...
X-RAY FLUORESCENCE BASED CHEMICAL COMPOSITION OF LADLE REFINERY FURNACE SLAG:...X-RAY FLUORESCENCE BASED CHEMICAL COMPOSITION OF LADLE REFINERY FURNACE SLAG:...
X-RAY FLUORESCENCE BASED CHEMICAL COMPOSITION OF LADLE REFINERY FURNACE SLAG:...IRJET Journal
 
Iron making
Iron makingIron making
Iron makingguddu_92
 
Module-1_Lesson-2.pdf
Module-1_Lesson-2.pdfModule-1_Lesson-2.pdf
Module-1_Lesson-2.pdfAskiRg
 
introduction of steel making types , classification
introduction of steel making types , classificationintroduction of steel making types , classification
introduction of steel making types , classificationMihirMandal7
 
IRJET- Experimental Investigation into the Effect of Austempering on Mech...
IRJET-  	  Experimental Investigation into the Effect of Austempering on Mech...IRJET-  	  Experimental Investigation into the Effect of Austempering on Mech...
IRJET- Experimental Investigation into the Effect of Austempering on Mech...IRJET Journal
 
Steel and cast iron ( application ,types and properties )
Steel and cast iron ( application ,types and properties )Steel and cast iron ( application ,types and properties )
Steel and cast iron ( application ,types and properties )Eng.Ahmed Samy
 

Ähnlich wie The International Journal of Engineering and Science (The IJES) (20)

Steel (construction material )
Steel (construction material )Steel (construction material )
Steel (construction material )
 
AMM - UNIT 1.pdf
AMM - UNIT 1.pdfAMM - UNIT 1.pdf
AMM - UNIT 1.pdf
 
Comparative Study on the High-Stress Abrasive Wear Behaviour of Zinc and Copp...
Comparative Study on the High-Stress Abrasive Wear Behaviour of Zinc and Copp...Comparative Study on the High-Stress Abrasive Wear Behaviour of Zinc and Copp...
Comparative Study on the High-Stress Abrasive Wear Behaviour of Zinc and Copp...
 
Studies on Corrosion Characteristics of Carbon Steel Exposed to Na2CO3, Na2SO...
Studies on Corrosion Characteristics of Carbon Steel Exposed to Na2CO3, Na2SO...Studies on Corrosion Characteristics of Carbon Steel Exposed to Na2CO3, Na2SO...
Studies on Corrosion Characteristics of Carbon Steel Exposed to Na2CO3, Na2SO...
 
Heat treatment course material
Heat treatment course materialHeat treatment course material
Heat treatment course material
 
Materialtechnologyforfertilizersindustries
MaterialtechnologyforfertilizersindustriesMaterialtechnologyforfertilizersindustries
Materialtechnologyforfertilizersindustries
 
How we can use ECOrrosion positivelyin our life
How we can use ECOrrosion positivelyin our lifeHow we can use ECOrrosion positivelyin our life
How we can use ECOrrosion positivelyin our life
 
Corrosion assessment & recommendations
Corrosion assessment & recommendationsCorrosion assessment & recommendations
Corrosion assessment & recommendations
 
Dk4301657662
Dk4301657662Dk4301657662
Dk4301657662
 
X-RAY FLUORESCENCE BASED CHEMICAL COMPOSITION OF LADLE REFINERY FURNACE SLAG:...
X-RAY FLUORESCENCE BASED CHEMICAL COMPOSITION OF LADLE REFINERY FURNACE SLAG:...X-RAY FLUORESCENCE BASED CHEMICAL COMPOSITION OF LADLE REFINERY FURNACE SLAG:...
X-RAY FLUORESCENCE BASED CHEMICAL COMPOSITION OF LADLE REFINERY FURNACE SLAG:...
 
J012275461
J012275461J012275461
J012275461
 
Iron making
Iron makingIron making
Iron making
 
Module-1_Lesson-2.pdf
Module-1_Lesson-2.pdfModule-1_Lesson-2.pdf
Module-1_Lesson-2.pdf
 
introduction of steel making types , classification
introduction of steel making types , classificationintroduction of steel making types , classification
introduction of steel making types , classification
 
Welding Coating.pdf
Welding Coating.pdfWelding Coating.pdf
Welding Coating.pdf
 
IRJET- Experimental Investigation into the Effect of Austempering on Mech...
IRJET-  	  Experimental Investigation into the Effect of Austempering on Mech...IRJET-  	  Experimental Investigation into the Effect of Austempering on Mech...
IRJET- Experimental Investigation into the Effect of Austempering on Mech...
 
Steel and cast iron ( application ,types and properties )
Steel and cast iron ( application ,types and properties )Steel and cast iron ( application ,types and properties )
Steel and cast iron ( application ,types and properties )
 
Aluminium and Its alloys.pptx
Aluminium and Its alloys.pptxAluminium and Its alloys.pptx
Aluminium and Its alloys.pptx
 
F05214252
F05214252F05214252
F05214252
 
Metals
MetalsMetals
Metals
 

Kürzlich hochgeladen

Famous Olympic Siblings from the 21st Century
Famous Olympic Siblings from the 21st CenturyFamous Olympic Siblings from the 21st Century
Famous Olympic Siblings from the 21st Centuryrwgiffor
 
Call Girls In Noida 959961⊹3876 Independent Escort Service Noida
Call Girls In Noida 959961⊹3876 Independent Escort Service NoidaCall Girls In Noida 959961⊹3876 Independent Escort Service Noida
Call Girls In Noida 959961⊹3876 Independent Escort Service Noidadlhescort
 
Cheap Rate Call Girls In Noida Sector 62 Metro 959961乂3876
Cheap Rate Call Girls In Noida Sector 62 Metro 959961乂3876Cheap Rate Call Girls In Noida Sector 62 Metro 959961乂3876
Cheap Rate Call Girls In Noida Sector 62 Metro 959961乂3876dlhescort
 
SEO Case Study: How I Increased SEO Traffic & Ranking by 50-60% in 6 Months
SEO Case Study: How I Increased SEO Traffic & Ranking by 50-60%  in 6 MonthsSEO Case Study: How I Increased SEO Traffic & Ranking by 50-60%  in 6 Months
SEO Case Study: How I Increased SEO Traffic & Ranking by 50-60% in 6 MonthsIndeedSEO
 
👉Chandigarh Call Girls 👉9878799926👉Just Call👉Chandigarh Call Girl In Chandiga...
👉Chandigarh Call Girls 👉9878799926👉Just Call👉Chandigarh Call Girl In Chandiga...👉Chandigarh Call Girls 👉9878799926👉Just Call👉Chandigarh Call Girl In Chandiga...
👉Chandigarh Call Girls 👉9878799926👉Just Call👉Chandigarh Call Girl In Chandiga...rajveerescorts2022
 
Phases of Negotiation .pptx
 Phases of Negotiation .pptx Phases of Negotiation .pptx
Phases of Negotiation .pptxnandhinijagan9867
 
Falcon Invoice Discounting: Unlock Your Business Potential
Falcon Invoice Discounting: Unlock Your Business PotentialFalcon Invoice Discounting: Unlock Your Business Potential
Falcon Invoice Discounting: Unlock Your Business PotentialFalcon investment
 
Call Girls Electronic City Just Call 👗 7737669865 👗 Top Class Call Girl Servi...
Call Girls Electronic City Just Call 👗 7737669865 👗 Top Class Call Girl Servi...Call Girls Electronic City Just Call 👗 7737669865 👗 Top Class Call Girl Servi...
Call Girls Electronic City Just Call 👗 7737669865 👗 Top Class Call Girl Servi...amitlee9823
 
Falcon Invoice Discounting: Empowering Your Business Growth
Falcon Invoice Discounting: Empowering Your Business GrowthFalcon Invoice Discounting: Empowering Your Business Growth
Falcon Invoice Discounting: Empowering Your Business GrowthFalcon investment
 
Russian Call Girls In Rajiv Chowk Gurgaon ❤️8448577510 ⊹Best Escorts Service ...
Russian Call Girls In Rajiv Chowk Gurgaon ❤️8448577510 ⊹Best Escorts Service ...Russian Call Girls In Rajiv Chowk Gurgaon ❤️8448577510 ⊹Best Escorts Service ...
Russian Call Girls In Rajiv Chowk Gurgaon ❤️8448577510 ⊹Best Escorts Service ...lizamodels9
 
Al Mizhar Dubai Escorts +971561403006 Escorts Service In Al Mizhar
Al Mizhar Dubai Escorts +971561403006 Escorts Service In Al MizharAl Mizhar Dubai Escorts +971561403006 Escorts Service In Al Mizhar
Al Mizhar Dubai Escorts +971561403006 Escorts Service In Al Mizharallensay1
 
Call Girls in Delhi, Escort Service Available 24x7 in Delhi 959961-/-3876
Call Girls in Delhi, Escort Service Available 24x7 in Delhi 959961-/-3876Call Girls in Delhi, Escort Service Available 24x7 in Delhi 959961-/-3876
Call Girls in Delhi, Escort Service Available 24x7 in Delhi 959961-/-3876dlhescort
 
Eluru Call Girls Service ☎ ️93326-06886 ❤️‍🔥 Enjoy 24/7 Escort Service
Eluru Call Girls Service ☎ ️93326-06886 ❤️‍🔥 Enjoy 24/7 Escort ServiceEluru Call Girls Service ☎ ️93326-06886 ❤️‍🔥 Enjoy 24/7 Escort Service
Eluru Call Girls Service ☎ ️93326-06886 ❤️‍🔥 Enjoy 24/7 Escort ServiceDamini Dixit
 
Marel Q1 2024 Investor Presentation from May 8, 2024
Marel Q1 2024 Investor Presentation from May 8, 2024Marel Q1 2024 Investor Presentation from May 8, 2024
Marel Q1 2024 Investor Presentation from May 8, 2024Marel
 
Call Girls From Pari Chowk Greater Noida ❤️8448577510 ⊹Best Escorts Service I...
Call Girls From Pari Chowk Greater Noida ❤️8448577510 ⊹Best Escorts Service I...Call Girls From Pari Chowk Greater Noida ❤️8448577510 ⊹Best Escorts Service I...
Call Girls From Pari Chowk Greater Noida ❤️8448577510 ⊹Best Escorts Service I...lizamodels9
 
Russian Call Girls In Gurgaon ❤️8448577510 ⊹Best Escorts Service In 24/7 Delh...
Russian Call Girls In Gurgaon ❤️8448577510 ⊹Best Escorts Service In 24/7 Delh...Russian Call Girls In Gurgaon ❤️8448577510 ⊹Best Escorts Service In 24/7 Delh...
Russian Call Girls In Gurgaon ❤️8448577510 ⊹Best Escorts Service In 24/7 Delh...lizamodels9
 
Falcon Invoice Discounting: The best investment platform in india for investors
Falcon Invoice Discounting: The best investment platform in india for investorsFalcon Invoice Discounting: The best investment platform in india for investors
Falcon Invoice Discounting: The best investment platform in india for investorsFalcon Invoice Discounting
 
Call Girls Kengeri Satellite Town Just Call 👗 7737669865 👗 Top Class Call Gir...
Call Girls Kengeri Satellite Town Just Call 👗 7737669865 👗 Top Class Call Gir...Call Girls Kengeri Satellite Town Just Call 👗 7737669865 👗 Top Class Call Gir...
Call Girls Kengeri Satellite Town Just Call 👗 7737669865 👗 Top Class Call Gir...amitlee9823
 
Call Girls From Raj Nagar Extension Ghaziabad❤️8448577510 ⊹Best Escorts Servi...
Call Girls From Raj Nagar Extension Ghaziabad❤️8448577510 ⊹Best Escorts Servi...Call Girls From Raj Nagar Extension Ghaziabad❤️8448577510 ⊹Best Escorts Servi...
Call Girls From Raj Nagar Extension Ghaziabad❤️8448577510 ⊹Best Escorts Servi...lizamodels9
 

Kürzlich hochgeladen (20)

Famous Olympic Siblings from the 21st Century
Famous Olympic Siblings from the 21st CenturyFamous Olympic Siblings from the 21st Century
Famous Olympic Siblings from the 21st Century
 
Call Girls In Noida 959961⊹3876 Independent Escort Service Noida
Call Girls In Noida 959961⊹3876 Independent Escort Service NoidaCall Girls In Noida 959961⊹3876 Independent Escort Service Noida
Call Girls In Noida 959961⊹3876 Independent Escort Service Noida
 
Cheap Rate Call Girls In Noida Sector 62 Metro 959961乂3876
Cheap Rate Call Girls In Noida Sector 62 Metro 959961乂3876Cheap Rate Call Girls In Noida Sector 62 Metro 959961乂3876
Cheap Rate Call Girls In Noida Sector 62 Metro 959961乂3876
 
SEO Case Study: How I Increased SEO Traffic & Ranking by 50-60% in 6 Months
SEO Case Study: How I Increased SEO Traffic & Ranking by 50-60%  in 6 MonthsSEO Case Study: How I Increased SEO Traffic & Ranking by 50-60%  in 6 Months
SEO Case Study: How I Increased SEO Traffic & Ranking by 50-60% in 6 Months
 
Falcon Invoice Discounting platform in india
Falcon Invoice Discounting platform in indiaFalcon Invoice Discounting platform in india
Falcon Invoice Discounting platform in india
 
👉Chandigarh Call Girls 👉9878799926👉Just Call👉Chandigarh Call Girl In Chandiga...
👉Chandigarh Call Girls 👉9878799926👉Just Call👉Chandigarh Call Girl In Chandiga...👉Chandigarh Call Girls 👉9878799926👉Just Call👉Chandigarh Call Girl In Chandiga...
👉Chandigarh Call Girls 👉9878799926👉Just Call👉Chandigarh Call Girl In Chandiga...
 
Phases of Negotiation .pptx
 Phases of Negotiation .pptx Phases of Negotiation .pptx
Phases of Negotiation .pptx
 
Falcon Invoice Discounting: Unlock Your Business Potential
Falcon Invoice Discounting: Unlock Your Business PotentialFalcon Invoice Discounting: Unlock Your Business Potential
Falcon Invoice Discounting: Unlock Your Business Potential
 
Call Girls Electronic City Just Call 👗 7737669865 👗 Top Class Call Girl Servi...
Call Girls Electronic City Just Call 👗 7737669865 👗 Top Class Call Girl Servi...Call Girls Electronic City Just Call 👗 7737669865 👗 Top Class Call Girl Servi...
Call Girls Electronic City Just Call 👗 7737669865 👗 Top Class Call Girl Servi...
 
Falcon Invoice Discounting: Empowering Your Business Growth
Falcon Invoice Discounting: Empowering Your Business GrowthFalcon Invoice Discounting: Empowering Your Business Growth
Falcon Invoice Discounting: Empowering Your Business Growth
 
Russian Call Girls In Rajiv Chowk Gurgaon ❤️8448577510 ⊹Best Escorts Service ...
Russian Call Girls In Rajiv Chowk Gurgaon ❤️8448577510 ⊹Best Escorts Service ...Russian Call Girls In Rajiv Chowk Gurgaon ❤️8448577510 ⊹Best Escorts Service ...
Russian Call Girls In Rajiv Chowk Gurgaon ❤️8448577510 ⊹Best Escorts Service ...
 
Al Mizhar Dubai Escorts +971561403006 Escorts Service In Al Mizhar
Al Mizhar Dubai Escorts +971561403006 Escorts Service In Al MizharAl Mizhar Dubai Escorts +971561403006 Escorts Service In Al Mizhar
Al Mizhar Dubai Escorts +971561403006 Escorts Service In Al Mizhar
 
Call Girls in Delhi, Escort Service Available 24x7 in Delhi 959961-/-3876
Call Girls in Delhi, Escort Service Available 24x7 in Delhi 959961-/-3876Call Girls in Delhi, Escort Service Available 24x7 in Delhi 959961-/-3876
Call Girls in Delhi, Escort Service Available 24x7 in Delhi 959961-/-3876
 
Eluru Call Girls Service ☎ ️93326-06886 ❤️‍🔥 Enjoy 24/7 Escort Service
Eluru Call Girls Service ☎ ️93326-06886 ❤️‍🔥 Enjoy 24/7 Escort ServiceEluru Call Girls Service ☎ ️93326-06886 ❤️‍🔥 Enjoy 24/7 Escort Service
Eluru Call Girls Service ☎ ️93326-06886 ❤️‍🔥 Enjoy 24/7 Escort Service
 
Marel Q1 2024 Investor Presentation from May 8, 2024
Marel Q1 2024 Investor Presentation from May 8, 2024Marel Q1 2024 Investor Presentation from May 8, 2024
Marel Q1 2024 Investor Presentation from May 8, 2024
 
Call Girls From Pari Chowk Greater Noida ❤️8448577510 ⊹Best Escorts Service I...
Call Girls From Pari Chowk Greater Noida ❤️8448577510 ⊹Best Escorts Service I...Call Girls From Pari Chowk Greater Noida ❤️8448577510 ⊹Best Escorts Service I...
Call Girls From Pari Chowk Greater Noida ❤️8448577510 ⊹Best Escorts Service I...
 
Russian Call Girls In Gurgaon ❤️8448577510 ⊹Best Escorts Service In 24/7 Delh...
Russian Call Girls In Gurgaon ❤️8448577510 ⊹Best Escorts Service In 24/7 Delh...Russian Call Girls In Gurgaon ❤️8448577510 ⊹Best Escorts Service In 24/7 Delh...
Russian Call Girls In Gurgaon ❤️8448577510 ⊹Best Escorts Service In 24/7 Delh...
 
Falcon Invoice Discounting: The best investment platform in india for investors
Falcon Invoice Discounting: The best investment platform in india for investorsFalcon Invoice Discounting: The best investment platform in india for investors
Falcon Invoice Discounting: The best investment platform in india for investors
 
Call Girls Kengeri Satellite Town Just Call 👗 7737669865 👗 Top Class Call Gir...
Call Girls Kengeri Satellite Town Just Call 👗 7737669865 👗 Top Class Call Gir...Call Girls Kengeri Satellite Town Just Call 👗 7737669865 👗 Top Class Call Gir...
Call Girls Kengeri Satellite Town Just Call 👗 7737669865 👗 Top Class Call Gir...
 
Call Girls From Raj Nagar Extension Ghaziabad❤️8448577510 ⊹Best Escorts Servi...
Call Girls From Raj Nagar Extension Ghaziabad❤️8448577510 ⊹Best Escorts Servi...Call Girls From Raj Nagar Extension Ghaziabad❤️8448577510 ⊹Best Escorts Servi...
Call Girls From Raj Nagar Extension Ghaziabad❤️8448577510 ⊹Best Escorts Servi...
 

The International Journal of Engineering and Science (The IJES)

  • 1. The International Journal Of Engineering And Science (IJES) ||Volume|| 2 ||Issue|| 11 ||Pages|| 18-24 ||2013|| ISSN (e): 2319 – 1813 ISSN (p): 2319 – 1805 Corrosion Properties of Plain Carbon Steels Engr Dr A.C Uzorh Head of Department, Mechanical Engineering Department Federal University of Technoloy Owerri PMB 1526 Owerri, Imo State, Nigeria. ----------------------------------------------------------ABSTRACT----------------------------------------------------------This paper looks at the corrosion characteristics of two grades of plain carbon steels of Ajaokuta steel company limited, namely, DIN 35-2 (Ribbed rod) and DIN 37-2 (plain rod). In three environments: Salt solution, Tap water and Moist soil. The company is located in Northern Nigeria. The corrosion characteristics of these two grades of plain carbon steel were studied under cold work condition and as rolled or untreated condition in the aforementioned media for a period of 22 days. Result obtained show that corrosion rates increases with increasing degree of cold work. In addition, it was found that corrosion rates of these products vary in the different corroding media with moist soil having the highest corrosive ability, followed by tap water and then 3% by weight of sodium chloride salt solution. Also the rib rod samples essentially corroded more than the plain rod samples in these various environments. Keywords: Corrosion, Plain Carbon Steels, Cold work, ------------------------------------------------------------------------------------------------------------ ---------------------------Date of Submission: 11 March, 2013 Date of Acceptance: 10, November 2013 -------------------------------------------------------------------------------------------------------- -------------------------------- I. INTRODUCTION Corrosion is recognized as a major problem both in developed and developing nations of the world. Millions of naira are being spent every year to control tosses of corrosion. With the added interest of steel technology and steel production in Nigeria, it is of paramount importace that thorough studies and investigations be carried out to estimate how these steel products behave in use. In this respect, their corrosion properties are of paramount importance. This paper looks at the corrosion properties of steels produced by Ajaokuta Steel company limited in different corroding environments namely: tap water, moist soil and 3% by weight of sodium chloride solution. Three percent of sodium chloride was used because its corrosive ability had been studied and known. Also salt solution stimulates the natural sea water in the laboratory because sea water in the laboratory does not truly represent the natural environment. This is also a consequence of the changes that occur in it on storage. Majorly the research will dwell on the two common known steels: 1) 2) Plain carbon steel Alloy steels (UHLIG+, H.H. 1963) Experiment is carried out on plain carbon steel because they are the most common sued steels in the industries. Plain carbon steels are divided into three groups: 1) 2) 3) low carbon steel medium carbon steel high carbon steels Steel – Carbon Steel It is an alloy of iron and carbon, with carbon content up to maximum of 1.5 – 2.0%. The carbon occurs in the form of iron carbide, because of its ability to increase the hardness and strength of the steel. Other certain elements like silicon, phosphorus, sulphur and manganese are also present in greater or lesser amount to impart certain amount of desirable properties to it. Most of the steels produced recently is the plain carbon steel or carbon steel. A carbon steel is defined as a steel which has its properties mainly due to its carbon content and does not contain more than 0.5% of silicon and 1.5% of manganese. (R.S Khurmi, J.K. Gupta 2005) (DEUTCHMAN, A.D. et al 1975). The plain steels are usually classified in their carbon content, the commonest of the range being mild steel carbon content. (W.A.J. Champion 1972). www.theijes.com The IJES Page 18
  • 2. Corrosion Properties of Plain Carbon Steels... APPLICATIONS OF CARBON STEELS (Chapman 1985) CARBON % Dead mild 0.1-0.125 Mild (low) 0.15-0.3 0.3-0.5 (0.05% - 0.30) Medium carbon (0.5 – 0.7) 0.7 – 0.9 (0.3% - 0.5%) High carbon (0.9-1.1) 1.1 – 1.4 (0.50% - 2.0%) USES Wire rod, thin sheets, solid drawn tubes, etc Boiler plates, bridge work, structural sections, drop forgings, general workshop purposes. Axes, drop forging, high tensile tubes and wire agricultural tools. Springs, locomotive tyres, large forging dies, wire ropes, hammers and snaps for riveters. Springs, small forging dies, spear blades, cold setts, wood chisels. Cold chisels, press dies, punches, secrewing dies, wood working tools axes, picks. Razors, hand files, drills,gauges, metal-cutting tools. This research paper is expected to help us understand how steel products of Ajaokuta Steel company and other related steel products corrode in different environments. It will also assist in finding means of minimizing or even preventing corrosion for it is said that “an ounce of prevention is worth a pound a pound of cure”. Or better say “prevention is better than cure”. Plain Carbon Steel The two types of carbon steels are plain carbon steel and alloy steel. Plain carbon steel is one which contains in addition to carbon and iron certain elements notably manganese, phosphorus, supphur and silicon in small quantities. It may also contain traces of elements like: copper, boron, cobalt and so on. Plain carbon steel is divided into three groups: 1) low carbon steel 2) medium carbon steel 3) high carbon steel (YOUNG, J.F.1982 Materials and Processes). Hot And Cold Working Of Plain Carbon Steel Rolling , forging, drawing, compression and extrusion and typical methods by which metals are worked especially steels have great effects on their mechanical and metallurgical properties. Cold working refers to the act of permanently deforming a cold metal. The term cold is relative. Even room temperature may be hot for such metals i.e as lead. A metal is said to be cold when it is worked at a temperature below recrystallization temperature but below the melting or boiling point is termed hot working. Metals are subjected to mechanical working for two general purposes: a) To reduce the original block or slug of metal approximately to the finished dimension of the part or mill form, thereby saving material, machining cost and time. b) To improve the mechanical properties of the material thoroughly Definition of Corrosion Corrosion may be defined broadly as the destruction or deterioration of metal by direct chemical and electro-chemical reaction with its environment. Most simply stated, metallic corrosion is the reverse of electroplating. The metal being corroded forms the anode while the cathode is that being electroplated. Metallic corrosion occurs because in many environment most metals are not inherently stable and tend to revert to some more stable combination of which the metallic ores as found in nature are familiar examples. Factors Influencing Corrosion Of Plain Carbon Steels Generally, the factors affecting the rate of corrosion of plain carbon steels are either material dependent or environment-dependent or a combination of both . Some of the factors which are associated mainly with metals are: 1) Over voltage of metal on the hydrogen. 2) Chemical and physical homogeneity of the metal surface. 3) Inherent ability to form an insoluble protective film 4) Hydrogen ion Activity (PH) in the solution 5) Influence of oxygen in the solution adjancent to the metal 6) Rate of flow of solution in contact with metal www.theijes.com The IJES Page 19
  • 3. Corrosion Properties of Plain Carbon Steels... Significance of Corrosion Corrosion has a lot of significance economically, socially and otherwise. This led J.M. West to write, "Corrosion kills people, waste resources and cost money we can ill afford". But except for a few corrosion reactions which are of practical importance for example, the corrosion of metallic lead, the effects of corrosion are nothing to write home about. Some of the disadvantage of corrosion includes: (a) (b) (c) (d) Wastage of material, money, time and man power due to over design, because of corrosion. Contamination of products eg damage of entire batch of soap by a corroded copper Cost of replacing corroded structure or components Loss of products for example oil or gas losses in corroded pipes. II. METHODOLOGY In this chapter, the focus includes methods and techniques adopted as well as the materials used for this study. This contains material used, working samples adopted and relevant carbon test carried out. III. DESCRIPTION Ajaokuta steel company limited was visited and some relevant materials were obtained for the study from this company. The material gotten from the company is Plain Carbon steel in the form of 16mm plain rolled rods ( steel grade: DIN 37-2) and 16mm ribbed rods (DIN 35-2). These rods were subsequently reduced to the required dimensions for the experiment using the lathe machine, grinding machine and hack saw. The diagram below shows reduction procedure adopted using the lathe machine. Mounting steel/rod on a lathe machine for reduction process Fig 3.2: Reduction process of steel/rod on a Lathe Machine After machining the materials they were further polished and cleaned with emery paper.The ribbed rods were reduced to 10mm in diameter and 20mm by length, this was done to ensure that ribs were completely removed for easier calculation of the exposed surface areas of the specimens. Then the plain rolled rods were reduced to 13mm in diameter and 20mm in length. All these measurements were done using the vernier callipers. These diameters were chosen in this manner wit diameter of samples being about one-half the length, to enable us compress the sample without them experiencing buckling effects. Specimens produced were 108: 56 plain rolled rod and 56 ribbed rod. www.theijes.com The IJES Page 20
  • 4. Corrosion Properties of Plain Carbon Steels... Cold Working Of Samples Coldworking of samples was achieved by compression. The compressive behaviours of each of the two different materials was determined using the 40-ion universal testing machine (UTM) in the laboratory. The testing was done to determine the different degrees of compression to which the material could be subjected without necessarily crushing them. 18 specimens of the ribbed rod were subjected to a compressive load of 7000kgf which compressed the length from 20mm to 17.8mm and enlarged the diameter from 10mm to 10.6mm. Also 18 more specimens of the ribbed rod were subjected to a compressive load of 7500kfg reducing the length of each of the 18 specimens from 20mm to approximately 15.7mm with diameter enlarged to 11.29mm. The percentage of cold work in the above two cases were calculated as follows: % cold work (%CW) = Change in cross-sectional area Original corss-sectional area %CW : 1 = 12.36% %CW : 2 = 27.5% Similarly, 18 plain rolled samples were given about 16% cold work by subjecting them to a compressive load of 7500kgf which compressed each of them from a length of 26mm to 22.4mm and increased their diameter approximately from 13mm to 1.401mm. In addition, 18 more samples of plain rolled rod were subjected to 9000kgf(compressive load) which gave about 30% cold work to each of them by reducing their length from 13mm to 1.482mm. Corrosion Tests Preparation Of Corroding Media Three types of corroding media were used, namely 1) Tap water – a sufficient quantity of weight 890 per bowl was used. The quantity was large enough for complete immersion of the corrosion specimen. 2) Moist soil – sandy loam soil of the following properties was used: PH value in H20=4.2, in Kcl=3.7 3) NACL solution – 3% by weight of NACL solution was used. The solution coomprised of distilled water and common salt(NaCl), mass of distilled water used per bowl was 790g. using the electronic weighing balance, mass of NaCl was 24.432g Corrosion Of Samples Eighteen plastic bowls were provied for eighteen groups of sample products. Specimens were weighed with electronic weighing balance, wih exposed surface area calculated. The compressed samples were again measured to determine the changes in lengths with new diameters calculated. The samples were arranged in three subscripts i.e tap water, salt solution and moist soil respectively. Care was taken not to allow samples to touch one another in order not to initiate galvanic action. As corrosion of samples proceeded day after day, distilled water was added to the salt solution or tap water solution to make up for losses due to evaporation. Decrease in the moisture conent was noticed by occasionally filling and reweighing the bowls to determine the loss in weight. Determination of Weight Lost No corrosion of sample was noticed the first day, corrosion was noticed the third day and care was taken to remove only the corrosion products. The samples were weighed with electronic weighing balance to determine their new weights. The weight loss of each of the samples was determined and recorded. The process of washing,drying,weighing,deterination of weight loss and recording was repeated for the 6 th, 10th, 14th, 18th, 22nd days. Experimental Results And Analysis The lengths, diameter and surface areas for the three groups of each of the two grades of plain carbon steel namely DIN 35-2(ribbed rod) and DIN37-2(plain rod) are given in the tables of three samples ( As Rolled Samples ARS; Compressed Samples with 1st degree of cold work CDW1 and Compressed samples with second degree of cold work CDW2) below: www.theijes.com The IJES Page 21
  • 5. Corrosion Properties of Plain Carbon Steels... Table 4.1 TYPICAL INITIAL PARAMETERS for Ribbed Rod (Din 35-2) Samples Group ARS CDW1 CDW2 Diameter,D (cm) 1.000 1.060 1.129 Length,L (cm) 2.00 1.78 1.57 Total Surface Area(cm2) 7.8540 7.6925 7.5708 Table 4.2 TYPICAL INITIAL PARAMETERS for Plain Rod (DIN37-2) Samples Group ARS CDW1 CDW2 Diameter,D (cm) 1.300 1.400 1.482 Length,L (cm) 2.60 2.24 2.00 Table 4.3 As Rolled Samples(ARS), Group 1 DAYS SAMPLES 0 3 6 10 14 18 22 A B C D E F G Material: Ribbed Rod INITIAL WEIGHT (kg) 12.110 12.115 11.987 12.105 12.082 11.985 12.110 WEIGHT LOSS (mg) 0 4 13 24 32 37 53 Table 4.4 Compressed Samples (CDW1), Group 2 DAYS SAMPLES 0 3 6 10 14 18 22 H I J K L M N INITIAL WEIGHT (kg) 12.154 11.943 12.148 12.001 12.110 12.010 12.154 0 12 19 28 37 48 57 SAMPLES 0 3 6 10 14 18 22 O P Q R S T U INITIAL WEIGHT (kg) 12.000 11.997 12.090 12.011 11.989 12.003 12.000 Table 4.6 As Rolled Samples(ARS), Group 4 DAYS SAMPLES 0 3 6 10 14 18 22 A2 B2 C2 D2 E2 F2 G2 www.theijes.com INITIAL WEIGHT (kg) 12.103 12.002 12.000 11.998 12.100 11.993 12.103 WEIGHT LOSS (mg) 0 13 22 32 41 50 60 0 3 9 18 28 33 37 The IJES WEIGHT LOSS/SURFACE AREA(mg/cm2) 0.0000 0.5093 1.6552 3.0558 4.0743 4.7109 6.7482 Medium: Tapwater EXPOSED SURFACE AREA(CM2) 7.6925 7.6925 7.6925 7.6925 7.6925 7.6925 7.6925 WEIGHT LOSS/SURFACE AREA(mg/cm2) 0.0000 1.5600 2.4699 3.6399 4.8271 6.2398 7.4098 Material: Ribbed Rod EXPOSED SURFACE AREA(CM2) 7.5708 7. 5708 7. 5708 7. 5708 7. 5708 7. 5708 7. 5708 Material: Ribbed Rod WEIGHT LOSS (mg) Medium: Tap Water EXPOSED SURFACE AREA(CM2) 7.854 7.854 7.854 7.854 7.854 7.854 7.854 Material: Ribbed Rod WEIGHT LOSS (mg) Table 4.5 Further Compressed Samples (CDW2), Group 3 Tapwater DAYS Total Surface Area(cm2) 13.2732 12.9422 12.7617 Medium: WEIGHT LOSS/SURFACE AREA(mg/cm2) 0.0000 1.7171 2.9059 4.2267 5.4155 6.6043 7.9252 Medium: NaCl Solution EXPOSED SURFACE AREA(CM2) 7.854 7.854 7.854 7.854 7.854 7.854 7.854 WEIGHT LOSS/SURFACE AREA(mg/cm2) 0.0000 0.3819 1.1459 2.2918 3.5651 4.2017 4.7110 Page 22
  • 6. Corrosion Properties of Plain Carbon Steels... Table 4.7 Compressed Samples (CDW1), Group 5 DAYS SAMPLES 0 3 6 10 14 18 22 H2 I2 J2 K2 L2 M2 N2 Table 4.8 DAYS 0 3 6 10 14 18 22 INITIAL WEIGHT (kg) 12.101 12.237 11.990 11.989 12.001 12.121 12.101 Material: Ribbed Rod WEIGHT LOSS (mg) 0 7 10 19 29 38 43 Medium: NaCl Solution EXPOSED SURFACE AREA(CM2) 7.6925 7.6925 7.6925 7.6925 7.6925 7.6925 7.6925 WEIGHT LOSS/SURFACE AREA(mg/cm2) 0.0000 0.0100 1.3000 2.4699 3.7699 4.9399 5.5899 Further Compressed Samples (CDW2), Group 6 Material: Ribbed Rod Medium: NaCl Solution SAMPLES INITIAL WEIGHT LOSS EXPOSED WEIGHT WEIGHT (mg) SURFACE LOSS/SURFACE (kg) AREA(CM2) AREA(mg/cm2) O2 12.172 0 7.5708 0.0000 P2 11.987 8 7. 5708 1.0567 Q2 11.998 13 7. 5708 1.7171 R2 12.003 21 7. 5708 2.7738 S2 11.997 31 7. 5708 4.0947 T2 12.013 40 7. 5708 5.2835 U2 12.172 46 7. 5708 6.0760 IV. OBSERVATION After the first day, each samples were surrounded by yellowish deposits evident in the tap water than salt solution. As days progress the deposits turned brown identified to be ferric hydroxide. Some shiny white patches of particles were suspected to be ferrous hydroxide formed due to the presence of insufficient oxygen. On withdrawal of specimed immersed in the moist soil, dark brown deposits of ferric hydroxide were noticed on them. The corroding media (tap water and salt solution) were observed to decrease continuously in volume due to evaporation of water. The decrease in the volume of media was evident from the ringed marks on the bowl inducating the original levels of the media. On washing of sample from salt solution and tap water, it was observed that the deposit on them were relatively easily removed except for the dark patches of samples which took quite some time, but samples of moist soil were not easily washed off. Analysis Of Result Based on the results deduced from the table, the analysis of result shows that on the whole, the ARS have the lowest corrosion rate, followed by CDW1 and the CDW2 having the highest corrosion rate. If a graph is plotted , the as rolled samples curve (ARS) will follow a gradual increase in corrosion attack on the first 6 days and then increase suddenly 4 days after followed by a gradual increase in the next 8 days and another increase in the last 4 days. Curves CDW1 and CDW2, has relatively high corrosion on the first 6 days. On the whole, the as rolled samples have the lowest corrosion rate , followed by CDW1 and with the CDW2 having the highest corrosion rate. Sudden change in the rate of corrosion attacks of the metals mentioned could be associated with the physical breakdown of the barrier films of the corrosion products which encourages corrosion attacks by exposing new surface area of the metals. In the case of moist soils the changes could be explained by the effect of making up of moisture loss which tends to promote corrosion. The marked low corrosion rates in the initial days mentioned especially for as rolled samples might be attributed to the effect of the surface finish of the samples. The as rolled samples have better surface finish of the samples. The as rolled samples have etter surface finish than the compressed samples. On the other hand the low corrosion rates experienced as the corrosion progressed after many days are likely indications that the protective films (corrosion products) accumulated over the past days tend to lower the rates of corrosion attack by not allowing enough contact between samples and corroding media. www.theijes.com The IJES Page 23
  • 7. Corrosion Properties of Plain Carbon Steels... The general trend obtained whereby the compressed samples corroded higher than their corresponding as rolled samples might be as a result of the increased rate of dissolution of the higher energy (strained) grains produced by the cold work effect by the corroding media. The fact that the samples coldworked to a higher degree corroded more than that cold worked to a lesser degree indicated that the increased rate of dissolution of the high energy (strained) grains is highest for them. V. CONCLUSION In general, the rate of corrosion of plain carbon steels is dependent on both the environmental conditions, structural and compositional properties of the steel. Within the limits of experimental error, conclusions drawn based on observations and result of the research are: 1) In corroding media for example, NaCl solution, tap water and moist soil , corrosion of plain carbon steel depends on the amount of oxygen dissolved in the media. 2) Among the three corroding media used in the experiment, moist soil has the highest corrosive ability followed by tap water and then NaCl solution. 3) The degree of cold water increases the corrosion of plain carbon steels of Ajaokuta steel company limited. 4) Plain carbon steels of Ajaokuta steel company limited as comparable to its counerparts from other places. Suggestions For Future Work a) To eliminate or reduce errors in future investigations of corrosion properties of materials by weght lost per unit area method, the following are sugested: b) The use of a better means of removing adherent corrosion products, say by the use of chemical means. c) An open building with the roof covered for better air circulation than the present laboratory should be provided for the experiment to allow better free circulation of air and real atmospheric condition to play their natural parts in corrosion process without rain necessarily disrupting the project set up. d) It is suggested that future researchers wishing to investigate properties of materials formulate mathematical relations existing between the extent of corrosio attack and time as well as investigation of corrosion properties of other steel products of Ajaokuta steel company limited and other local steel producing companies. Limitations Of Experimental Results The possible sources of errors are likely to be from: 1) The instument used: such errors include errors due to low sensitivity of instruments, faulty instruments etc 2) The method of preparing the samples by machining , grinding and cleaning with energy paper may not have ensured uniform surface finish and dimensions where necessary. Also in the compression process, the stress developed in the process may not have been uniformly distriuted. 3) The physical method of removing corrosion products can introduce errors, since the corrosion product may not be properly and completely removed. 4) The atmospheric condition that obtains in the laboratory may not compare favourably with that obtained in a better open place. Hence free circulation of air and real atmospheric conditions may not be allowed to play their natural part in the corrosion well enough. REFERENCES [1]. [2]. [3]. [4]. [5]. [6]. [7]. [8]. [9]. Chapman, F. A. (1985): Corrosion testing procedures 2nd Edition, Chapman and Hall Publishers, Incorporated, London. Duetchman, A.D. et al (1975): Machine Design, Theory and Practice, Collier Macmillian Publishers, (Inc) London. J.k Gupta. (2005) : 4th Edition, R.S. Khurmi Machine Design. West J.M. (1980) Basic corrosion and oxidation, Ellis Hordward Publishers, Manchester. Young, J.F. (1982): 2nd edition, John Wiley and Sons, New York. http://www.emeraldinsight.com/products/journals/journals.htm?id=acmm http://www.engineeringtoolbox.com/corrosion-d_986.html http://en.wikipedia.org/wiki/Corrosion http://www.corrosionprevention.org.uk/ www.theijes.com The IJES Page 24