General Origin of Defects
in Casting
• 1. Casting Design.
• 2. Technique of Manufacture
(Method).
• 3. Application of Technique
(Workmanship).
Defects Grouped According
to their Origin
1. Shaping faults arising in pouring.
2. Inclusions and sand defects.
3. Gas defects.
4. Shrinkage defects.
5. Contraction defects.
6. Dimensional errors.
7. Compositional errors and
segregation.
Shaping faults arising in
pouring.
• The liquid metal should satisfactorily
fill the mould cavity and develop a
smooth skin through intimate contact
with the mould surface.
• The type of defects that might arise
if this requirement is not met are:
Misrun; Shortrun; Cold laps; Cold
shuts.
Shaping faults arising in
pouring.
• Misrun or Shortrun: the metal
solidifies prematurely and some limb
or section of the casting is missing.
• Cold Laps: a less severe
manifestation of misrun.
• Cold shuts: the discontinuity extends
through the casting member.
Shaping faults arising in
pouring.
These defects appear due to the following
reasons:
Low metal temperature.
Excessive chilling from the mould face.
Too high moisture content in green sand.
A method developed for dry sand used in
conjunction with green sand.
Occurrence of rounded corners and edges
and a general lack of definition of sharp
features and fine mould detail.
Shrinkage Defects
• Shrinkage defects arise from failure
to compensate for liquid and
solidification contraction so their
occurrence is usually a symptom of
inadequate gating and risering
techniques.
• Types of shrinkage defects:
o Major shrinkage cavity.
o Discrete porosity:
o Sinks and surface punctures.
Shrinkage Defects
• Major Shrinkage Cavities
Appear in those alloys of short freezing
range i.e. solidify by skin formation.
• Discrete Porosity
The longer freezing range alloys are
subjected to scattered porosity,
susceptible alloys include: bronzes, gun
metals, and numerous light alloys and
phosphorous containing cast irons.
Chilling by inserting chills in the moulding
material is used to combat surface
porosity in these alloys.
Shrinkage Defects
• Sinks and surface punctures:
The solidified skins deform under
atmospheric pressure due to the
occurrence of low pressure
conditions within the casting.
This defect can be avoided by
ensuring access of atmospheric
pressure to the liquid metal in the
feeder head.
Contraction Defects
• Contraction occurs upon cooling from the solidus
to room temperature. Unlike the liquid and
solidification shrinkages, which can be
compensated by by influx of liquid, solid
contraction affects all linear dimensions of the
casting, hence standard pattern allowances are
made.
• However, under practical cooling conditions,
castings usually have thin and thick sections, so
they do not contract freely and the metal
develops cohesive strength to overcome
significant resistance or hindrance to contraction
which is offered by the mould or other parts of
the casting itself which vary in their thickness.
Contraction Defects
• Hot Tears:
Hot tears or pulls are one form of this
type of defect often located at junctions
where changes in section occur, as the thin
part cools more rapidly then the thick part
and when the thick parts cool and start to
contract they cannot contract freely
because the thin section has cooled enough
to become hard and rigid so the material
tears at the junction separating the thin
part from the thick part.
Gas Defects
• Defects of this type take the form
of internal blow holes, surface blows,
airlocks, surface or subcutaneous
pinholes or intergranular cavities.
Gas Defects
They result from:
• Entrapment of air during pouring.
• Evolution of water vapour on contact
between liquid metal and moulding
material.
• Precipitation during solidification as
a result of chemical reaction or
change in solubility.
Gas Defects
• Gases enter liquid metal during
melting as temperature increases
the solubility of gases in the liquid
increases, and vice versa.
• The sources of gases are either:
• mould gases,
• Gases evolving from the metal upon
solidification.
Gas Defects
The preventive measures are:
Melting precautions:
• preheating of charge materials to
evaporate surface moisture, also
preheating any material added to the
liquid bath during melting.
• Fast melting.
• Using protective fluxes.
Follow Melting
Precautions:
• Following proper melt treatment:
oxidation-deoxidation reactions.
• Maintaining the metal temperature as low
as possible.
• Drying and preheating all spouts, ladles,
shanks, and furnace tools.
• Vacuum melting if justifiable.
• Degasing molten metal: gas scavenging by
argon, nitrogen, or chlorine, or by vacuum
degasing for non-ferrous metals.
Inclusions and Sand
Defects
• Non-Metallic inclusions in castings
may be considered in two Min groups:
• Indigenous arising from reactions
within the melt (may not be regarded
as defects).
• Exogenous resulting from
entrainment of non-metallics during
pouring (dross, slag, flux residues, or
moulding material).
Inclusions and Sand
Defects
• Inclusions are frequently
concentrated at or immediately below
the upper surfaces of castings,
where they are revealed on machining
or after scaling in heat treatment. It
is advisable that the most important
faces be placed downwards.
Increased machining allowances are
usually made on top surfaces of
castings.
Inclusions and Sand
Defects
The types of these defects are:
• Erosion scabs: A rough projection on
the casting as sand is washed away.
• Expansion defect: results from
penetration of liquid meatal behind
the surface layer of the sand.
• Rat tail: Surface fissure or line
defect.
• Surface roughness and sand
Dimensional Errors
• Such errors can occur in pattern
making, moulding, and casting, or
fettling.
• Principal causes are misalignment of
mould parts and cores, mould
distortion, anomalous contraction and
distortion in cooling.
Compositional Errors and
Segregation
• The main causes for variation in composition from
desired one are:
 Melting losses.
 Incorrect furnace charge.
• Careful melting practice is essential.
• Segregation is unavoided (macro or micro) in cast
alloys.
• Homogenisation treatment is necessary for
castings and it eliminates concentration gradients
by diffusion.
SPHERICAL HOLESSPHERICAL HOLES
CO-gas Defects
Gas holes on top surface only, revealed by
machining.
More severe type of the gas hole defects shown
in previous figure with inclusion of slag
particles.
Form: on the top surface, revealed during machining – sometimes discovered underneath a core.
Causes:
•Low pouring temperature
•High Mn and S contents
•Dirty ladles, lacks of skimming, poor refractory quality
SPHERICAL HOLESSPHERICAL HOLES
Hydrogen Pinholing
Small, spherical holes with shiny surface occurring
just below casting surface
Shiny graphite film appearing on surface of
defect type shown in previous figures.
Form: small spherical holes on all faces of the casting adjacent to the mould – with shiny surfaces.
Causes:
•Contamination of iron with Al.
Form:
- Scrap
- Inoculates
•Too high moisture content in sand
•Too long runner system
SPHERICAL HOLESSPHERICAL HOLES
Nitrogen Defects
Occurrence of small spherical holes adjacent to core,
often revealed immediately after knockout
Form: small spherical holes (sometimes more elongated) adjacent to cores
Causes:
•Nitrogen containing binders
•Too much addition of resin
•Too high N2-content in resin
ROUNDED HOLESROUNDED HOLES
Shrinkage Defects
Surface depression occurring at hot spot
Form: surface sink often with exuded bead of metal inside them or small depressions at hot spots with associated subsurface hole
Causes:
• too low mold rigidity causes yielding under ferostatic or solidification pressures
• too high pouring temperature
• too low carbon content
ROUNDED HOLESROUNDED HOLES
Gas Blowholes from Cores, Molds, or Inserts
Blowholes in plate casting
Causes:
• Excessive moisture content of sand
• Vents of cores are blocked
• Cores are underbaked or with excessive binder content
• Rusty or contaminated chills (denseners) or chaplets
Blowholes in cored casting resulting from
metal entering core vent. The metal extracted
from the core vent is also shown.
IRREGULAR HOLESIRREGULAR HOLES
Shrinkage Defects
Micrograph illustrating dendritic form of
internal porosity
Form:
• open metal, often interconnected areas
• has a dendritic form
• generally occurs in the heavier sections or hot spots such as positions adjacent to ingates or risers
Causes:
• lack of mold rigidity
• high pouring temperature
• over inoculation
• high phosphorous content
IRREGULAR HOLESIRREGULAR HOLES
Gas Defects from Molten Iron
Form: discrete fissures rather than areas of interconnected open metal may be widely dispersed or more isolated
Causes:
• Too much gas content in molten iron
• The more widely dispersed holes are due to N2
• The more isolated cavities are due to high H2 - content
Widely dispersed fissure defects
Larger, isolated fissure defects

Weitere ähnliche Inhalte

Was ist angesagt?

Was ist angesagt? (20)

Casting defects
Casting defectsCasting defects
Casting defects
 
U2 p casting processes
U2 p casting processesU2 p casting processes
U2 p casting processes
 
Casting Defect and solidification (1).pdf
Casting Defect and solidification (1).pdfCasting Defect and solidification (1).pdf
Casting Defect and solidification (1).pdf
 
Advanced casting and welding
Advanced casting and weldingAdvanced casting and welding
Advanced casting and welding
 
Investment casting 1
Investment casting 1Investment casting 1
Investment casting 1
 
Metal casting ppt3
Metal casting ppt3Metal casting ppt3
Metal casting ppt3
 
Casting defects
Casting defectsCasting defects
Casting defects
 
Casting
CastingCasting
Casting
 
Semi Solid Metal Casting
Semi Solid Metal CastingSemi Solid Metal Casting
Semi Solid Metal Casting
 
Mould gating system for foundry and metal casting
Mould gating system for foundry and metal castingMould gating system for foundry and metal casting
Mould gating system for foundry and metal casting
 
Introduction to Casting
Introduction to CastingIntroduction to Casting
Introduction to Casting
 
Welding metallurgy
Welding metallurgyWelding metallurgy
Welding metallurgy
 
Defects
DefectsDefects
Defects
 
Metal casting process part 2
Metal casting process part 2Metal casting process part 2
Metal casting process part 2
 
Core type and applications (1.2)
Core type and applications (1.2)Core type and applications (1.2)
Core type and applications (1.2)
 
Heat treatment
Heat treatmentHeat treatment
Heat treatment
 
Heat affected zone
Heat affected zoneHeat affected zone
Heat affected zone
 
Metal Casting processes including pattern making and mold making,Patterns,Cas...
Metal Casting processes including pattern making and mold making,Patterns,Cas...Metal Casting processes including pattern making and mold making,Patterns,Cas...
Metal Casting processes including pattern making and mold making,Patterns,Cas...
 
Extrusion
ExtrusionExtrusion
Extrusion
 
Sand casting of metals - Gating system for sand casting mould
Sand casting of metals - Gating system for sand casting mouldSand casting of metals - Gating system for sand casting mould
Sand casting of metals - Gating system for sand casting mould
 

Andere mochten auch (7)

Corrosion Sl Part Two
Corrosion Sl Part TwoCorrosion Sl Part Two
Corrosion Sl Part Two
 
U3 p4 casting defects
U3 p4 casting defectsU3 p4 casting defects
U3 p4 casting defects
 
Casting procedures
Casting procedures Casting procedures
Casting procedures
 
Industrial gas turbine (air cooling & sealing sys) 5th
Industrial gas turbine (air cooling & sealing sys)   5thIndustrial gas turbine (air cooling & sealing sys)   5th
Industrial gas turbine (air cooling & sealing sys) 5th
 
Casing defects
Casing defectsCasing defects
Casing defects
 
DELMER-Lost wax Investment Casting Process
DELMER-Lost wax Investment Casting ProcessDELMER-Lost wax Investment Casting Process
DELMER-Lost wax Investment Casting Process
 
Investment Casting ppt
Investment Casting pptInvestment Casting ppt
Investment Casting ppt
 

Ähnlich wie Casting defects by yaser elkelawy

Defects and electroplating
Defects and electroplatingDefects and electroplating
Defects and electroplating
SAIFoundry
 
Me 328 welding metallurgy
Me 328 welding metallurgyMe 328 welding metallurgy
Me 328 welding metallurgy
Reandy Risky
 
Casting-Defects-ppt.pptx Casting-Defects _Casting-Defects _Casting-Defects _...
Casting-Defects-ppt.pptx  Casting-Defects _Casting-Defects _Casting-Defects _...Casting-Defects-ppt.pptx  Casting-Defects _Casting-Defects _Casting-Defects _...
Casting-Defects-ppt.pptx Casting-Defects _Casting-Defects _Casting-Defects _...
YoussefSameh20
 
Details of the Casting process is included in a single PPT
Details of the Casting process is included in a single PPTDetails of the Casting process is included in a single PPT
Details of the Casting process is included in a single PPT
AshutoshPattanaik12
 

Ähnlich wie Casting defects by yaser elkelawy (20)

Manufacturing process sessional casting defacts
Manufacturing process sessional casting defactsManufacturing process sessional casting defacts
Manufacturing process sessional casting defacts
 
Shubhma mp2
Shubhma mp2Shubhma mp2
Shubhma mp2
 
Failures in casting
Failures in castingFailures in casting
Failures in casting
 
Casting defects
Casting defectsCasting defects
Casting defects
 
Cracks in-welds
Cracks in-weldsCracks in-welds
Cracks in-welds
 
HOT CRACKS AND COLD CRACKS (Welding)
HOT CRACKS AND COLD CRACKS (Welding)HOT CRACKS AND COLD CRACKS (Welding)
HOT CRACKS AND COLD CRACKS (Welding)
 
Manufacturing processes
Manufacturing processesManufacturing processes
Manufacturing processes
 
Steps invoved in casting
Steps invoved in castingSteps invoved in casting
Steps invoved in casting
 
CASTING PPT
CASTING PPTCASTING PPT
CASTING PPT
 
Design Consideration For Casting
Design Consideration For CastingDesign Consideration For Casting
Design Consideration For Casting
 
Casting process
Casting processCasting process
Casting process
 
Special Casting Processes.pptx
Special Casting Processes.pptxSpecial Casting Processes.pptx
Special Casting Processes.pptx
 
Defects and electroplating
Defects and electroplatingDefects and electroplating
Defects and electroplating
 
Gating system :- CASTING PROCESSES
Gating system :- CASTING PROCESSESGating system :- CASTING PROCESSES
Gating system :- CASTING PROCESSES
 
IIIE SECTION A MANUFACTURING TECHNOLOGY NOTES : 10.CASTINGS AND ITS DEFECTS
IIIE SECTION A MANUFACTURING TECHNOLOGY NOTES : 10.CASTINGS AND ITS DEFECTSIIIE SECTION A MANUFACTURING TECHNOLOGY NOTES : 10.CASTINGS AND ITS DEFECTS
IIIE SECTION A MANUFACTURING TECHNOLOGY NOTES : 10.CASTINGS AND ITS DEFECTS
 
Me 328 welding metallurgy
Me 328 welding metallurgyMe 328 welding metallurgy
Me 328 welding metallurgy
 
Casting-Defects-ppt.pptx Casting-Defects _Casting-Defects _Casting-Defects _...
Casting-Defects-ppt.pptx  Casting-Defects _Casting-Defects _Casting-Defects _...Casting-Defects-ppt.pptx  Casting-Defects _Casting-Defects _Casting-Defects _...
Casting-Defects-ppt.pptx Casting-Defects _Casting-Defects _Casting-Defects _...
 
4525108.ppt
4525108.ppt4525108.ppt
4525108.ppt
 
Details of the Casting process is included in a single PPT
Details of the Casting process is included in a single PPTDetails of the Casting process is included in a single PPT
Details of the Casting process is included in a single PPT
 
Casting Defect.pptx
Casting Defect.pptxCasting Defect.pptx
Casting Defect.pptx
 

Kürzlich hochgeladen

Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...
Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...
Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...
Christo Ananth
 
Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...
Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...
Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...
Christo Ananth
 

Kürzlich hochgeladen (20)

Call Girls Pimpri Chinchwad Call Me 7737669865 Budget Friendly No Advance Boo...
Call Girls Pimpri Chinchwad Call Me 7737669865 Budget Friendly No Advance Boo...Call Girls Pimpri Chinchwad Call Me 7737669865 Budget Friendly No Advance Boo...
Call Girls Pimpri Chinchwad Call Me 7737669865 Budget Friendly No Advance Boo...
 
The Most Attractive Pune Call Girls Budhwar Peth 8250192130 Will You Miss Thi...
The Most Attractive Pune Call Girls Budhwar Peth 8250192130 Will You Miss Thi...The Most Attractive Pune Call Girls Budhwar Peth 8250192130 Will You Miss Thi...
The Most Attractive Pune Call Girls Budhwar Peth 8250192130 Will You Miss Thi...
 
(SHREYA) Chakan Call Girls Just Call 7001035870 [ Cash on Delivery ] Pune Esc...
(SHREYA) Chakan Call Girls Just Call 7001035870 [ Cash on Delivery ] Pune Esc...(SHREYA) Chakan Call Girls Just Call 7001035870 [ Cash on Delivery ] Pune Esc...
(SHREYA) Chakan Call Girls Just Call 7001035870 [ Cash on Delivery ] Pune Esc...
 
Processing & Properties of Floor and Wall Tiles.pptx
Processing & Properties of Floor and Wall Tiles.pptxProcessing & Properties of Floor and Wall Tiles.pptx
Processing & Properties of Floor and Wall Tiles.pptx
 
Introduction and different types of Ethernet.pptx
Introduction and different types of Ethernet.pptxIntroduction and different types of Ethernet.pptx
Introduction and different types of Ethernet.pptx
 
Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...
Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...
Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...
 
Call Girls Service Nagpur Tanvi Call 7001035870 Meet With Nagpur Escorts
Call Girls Service Nagpur Tanvi Call 7001035870 Meet With Nagpur EscortsCall Girls Service Nagpur Tanvi Call 7001035870 Meet With Nagpur Escorts
Call Girls Service Nagpur Tanvi Call 7001035870 Meet With Nagpur Escorts
 
High Profile Call Girls Nagpur Meera Call 7001035870 Meet With Nagpur Escorts
High Profile Call Girls Nagpur Meera Call 7001035870 Meet With Nagpur EscortsHigh Profile Call Girls Nagpur Meera Call 7001035870 Meet With Nagpur Escorts
High Profile Call Girls Nagpur Meera Call 7001035870 Meet With Nagpur Escorts
 
Java Programming :Event Handling(Types of Events)
Java Programming :Event Handling(Types of Events)Java Programming :Event Handling(Types of Events)
Java Programming :Event Handling(Types of Events)
 
ONLINE FOOD ORDER SYSTEM PROJECT REPORT.pdf
ONLINE FOOD ORDER SYSTEM PROJECT REPORT.pdfONLINE FOOD ORDER SYSTEM PROJECT REPORT.pdf
ONLINE FOOD ORDER SYSTEM PROJECT REPORT.pdf
 
Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...
Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...
Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...
 
UNIT - IV - Air Compressors and its Performance
UNIT - IV - Air Compressors and its PerformanceUNIT - IV - Air Compressors and its Performance
UNIT - IV - Air Compressors and its Performance
 
Porous Ceramics seminar and technical writing
Porous Ceramics seminar and technical writingPorous Ceramics seminar and technical writing
Porous Ceramics seminar and technical writing
 
University management System project report..pdf
University management System project report..pdfUniversity management System project report..pdf
University management System project report..pdf
 
Introduction to Multiple Access Protocol.pptx
Introduction to Multiple Access Protocol.pptxIntroduction to Multiple Access Protocol.pptx
Introduction to Multiple Access Protocol.pptx
 
(PRIYA) Rajgurunagar Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
(PRIYA) Rajgurunagar Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...(PRIYA) Rajgurunagar Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
(PRIYA) Rajgurunagar Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
 
Roadmap to Membership of RICS - Pathways and Routes
Roadmap to Membership of RICS - Pathways and RoutesRoadmap to Membership of RICS - Pathways and Routes
Roadmap to Membership of RICS - Pathways and Routes
 
Booking open Available Pune Call Girls Koregaon Park 6297143586 Call Hot Ind...
Booking open Available Pune Call Girls Koregaon Park  6297143586 Call Hot Ind...Booking open Available Pune Call Girls Koregaon Park  6297143586 Call Hot Ind...
Booking open Available Pune Call Girls Koregaon Park 6297143586 Call Hot Ind...
 
(ANJALI) Dange Chowk Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
(ANJALI) Dange Chowk Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...(ANJALI) Dange Chowk Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
(ANJALI) Dange Chowk Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
 
BSides Seattle 2024 - Stopping Ethan Hunt From Taking Your Data.pptx
BSides Seattle 2024 - Stopping Ethan Hunt From Taking Your Data.pptxBSides Seattle 2024 - Stopping Ethan Hunt From Taking Your Data.pptx
BSides Seattle 2024 - Stopping Ethan Hunt From Taking Your Data.pptx
 

Casting defects by yaser elkelawy

  • 1. CASTING DEFECTSCASTING DEFECTS By: yaser elkelawyBy: yaser elkelawy From: united company forFrom: united company for foundries.foundries.
  • 2. General Origin of Defects in Casting • 1. Casting Design. • 2. Technique of Manufacture (Method). • 3. Application of Technique (Workmanship).
  • 3. Defects Grouped According to their Origin 1. Shaping faults arising in pouring. 2. Inclusions and sand defects. 3. Gas defects. 4. Shrinkage defects. 5. Contraction defects. 6. Dimensional errors. 7. Compositional errors and segregation.
  • 4. Shaping faults arising in pouring. • The liquid metal should satisfactorily fill the mould cavity and develop a smooth skin through intimate contact with the mould surface. • The type of defects that might arise if this requirement is not met are: Misrun; Shortrun; Cold laps; Cold shuts.
  • 5. Shaping faults arising in pouring. • Misrun or Shortrun: the metal solidifies prematurely and some limb or section of the casting is missing. • Cold Laps: a less severe manifestation of misrun. • Cold shuts: the discontinuity extends through the casting member.
  • 6. Shaping faults arising in pouring. These defects appear due to the following reasons: Low metal temperature. Excessive chilling from the mould face. Too high moisture content in green sand. A method developed for dry sand used in conjunction with green sand. Occurrence of rounded corners and edges and a general lack of definition of sharp features and fine mould detail.
  • 7. Shrinkage Defects • Shrinkage defects arise from failure to compensate for liquid and solidification contraction so their occurrence is usually a symptom of inadequate gating and risering techniques. • Types of shrinkage defects: o Major shrinkage cavity. o Discrete porosity: o Sinks and surface punctures.
  • 8. Shrinkage Defects • Major Shrinkage Cavities Appear in those alloys of short freezing range i.e. solidify by skin formation. • Discrete Porosity The longer freezing range alloys are subjected to scattered porosity, susceptible alloys include: bronzes, gun metals, and numerous light alloys and phosphorous containing cast irons. Chilling by inserting chills in the moulding material is used to combat surface porosity in these alloys.
  • 9. Shrinkage Defects • Sinks and surface punctures: The solidified skins deform under atmospheric pressure due to the occurrence of low pressure conditions within the casting. This defect can be avoided by ensuring access of atmospheric pressure to the liquid metal in the feeder head.
  • 10. Contraction Defects • Contraction occurs upon cooling from the solidus to room temperature. Unlike the liquid and solidification shrinkages, which can be compensated by by influx of liquid, solid contraction affects all linear dimensions of the casting, hence standard pattern allowances are made. • However, under practical cooling conditions, castings usually have thin and thick sections, so they do not contract freely and the metal develops cohesive strength to overcome significant resistance or hindrance to contraction which is offered by the mould or other parts of the casting itself which vary in their thickness.
  • 11. Contraction Defects • Hot Tears: Hot tears or pulls are one form of this type of defect often located at junctions where changes in section occur, as the thin part cools more rapidly then the thick part and when the thick parts cool and start to contract they cannot contract freely because the thin section has cooled enough to become hard and rigid so the material tears at the junction separating the thin part from the thick part.
  • 12.
  • 13.
  • 14.
  • 15.
  • 16.
  • 17. Gas Defects • Defects of this type take the form of internal blow holes, surface blows, airlocks, surface or subcutaneous pinholes or intergranular cavities.
  • 18. Gas Defects They result from: • Entrapment of air during pouring. • Evolution of water vapour on contact between liquid metal and moulding material. • Precipitation during solidification as a result of chemical reaction or change in solubility.
  • 19. Gas Defects • Gases enter liquid metal during melting as temperature increases the solubility of gases in the liquid increases, and vice versa. • The sources of gases are either: • mould gases, • Gases evolving from the metal upon solidification.
  • 20. Gas Defects The preventive measures are: Melting precautions: • preheating of charge materials to evaporate surface moisture, also preheating any material added to the liquid bath during melting. • Fast melting. • Using protective fluxes.
  • 21. Follow Melting Precautions: • Following proper melt treatment: oxidation-deoxidation reactions. • Maintaining the metal temperature as low as possible. • Drying and preheating all spouts, ladles, shanks, and furnace tools. • Vacuum melting if justifiable. • Degasing molten metal: gas scavenging by argon, nitrogen, or chlorine, or by vacuum degasing for non-ferrous metals.
  • 22. Inclusions and Sand Defects • Non-Metallic inclusions in castings may be considered in two Min groups: • Indigenous arising from reactions within the melt (may not be regarded as defects). • Exogenous resulting from entrainment of non-metallics during pouring (dross, slag, flux residues, or moulding material).
  • 23. Inclusions and Sand Defects • Inclusions are frequently concentrated at or immediately below the upper surfaces of castings, where they are revealed on machining or after scaling in heat treatment. It is advisable that the most important faces be placed downwards. Increased machining allowances are usually made on top surfaces of castings.
  • 24. Inclusions and Sand Defects The types of these defects are: • Erosion scabs: A rough projection on the casting as sand is washed away. • Expansion defect: results from penetration of liquid meatal behind the surface layer of the sand. • Rat tail: Surface fissure or line defect. • Surface roughness and sand
  • 25. Dimensional Errors • Such errors can occur in pattern making, moulding, and casting, or fettling. • Principal causes are misalignment of mould parts and cores, mould distortion, anomalous contraction and distortion in cooling.
  • 26.
  • 27.
  • 28. Compositional Errors and Segregation • The main causes for variation in composition from desired one are:  Melting losses.  Incorrect furnace charge. • Careful melting practice is essential. • Segregation is unavoided (macro or micro) in cast alloys. • Homogenisation treatment is necessary for castings and it eliminates concentration gradients by diffusion.
  • 29. SPHERICAL HOLESSPHERICAL HOLES CO-gas Defects Gas holes on top surface only, revealed by machining. More severe type of the gas hole defects shown in previous figure with inclusion of slag particles. Form: on the top surface, revealed during machining – sometimes discovered underneath a core. Causes: •Low pouring temperature •High Mn and S contents •Dirty ladles, lacks of skimming, poor refractory quality
  • 30. SPHERICAL HOLESSPHERICAL HOLES Hydrogen Pinholing Small, spherical holes with shiny surface occurring just below casting surface Shiny graphite film appearing on surface of defect type shown in previous figures. Form: small spherical holes on all faces of the casting adjacent to the mould – with shiny surfaces. Causes: •Contamination of iron with Al. Form: - Scrap - Inoculates •Too high moisture content in sand •Too long runner system
  • 31. SPHERICAL HOLESSPHERICAL HOLES Nitrogen Defects Occurrence of small spherical holes adjacent to core, often revealed immediately after knockout Form: small spherical holes (sometimes more elongated) adjacent to cores Causes: •Nitrogen containing binders •Too much addition of resin •Too high N2-content in resin
  • 32. ROUNDED HOLESROUNDED HOLES Shrinkage Defects Surface depression occurring at hot spot Form: surface sink often with exuded bead of metal inside them or small depressions at hot spots with associated subsurface hole Causes: • too low mold rigidity causes yielding under ferostatic or solidification pressures • too high pouring temperature • too low carbon content
  • 33. ROUNDED HOLESROUNDED HOLES Gas Blowholes from Cores, Molds, or Inserts Blowholes in plate casting Causes: • Excessive moisture content of sand • Vents of cores are blocked • Cores are underbaked or with excessive binder content • Rusty or contaminated chills (denseners) or chaplets Blowholes in cored casting resulting from metal entering core vent. The metal extracted from the core vent is also shown.
  • 34. IRREGULAR HOLESIRREGULAR HOLES Shrinkage Defects Micrograph illustrating dendritic form of internal porosity Form: • open metal, often interconnected areas • has a dendritic form • generally occurs in the heavier sections or hot spots such as positions adjacent to ingates or risers Causes: • lack of mold rigidity • high pouring temperature • over inoculation • high phosphorous content
  • 35. IRREGULAR HOLESIRREGULAR HOLES Gas Defects from Molten Iron Form: discrete fissures rather than areas of interconnected open metal may be widely dispersed or more isolated Causes: • Too much gas content in molten iron • The more widely dispersed holes are due to N2 • The more isolated cavities are due to high H2 - content Widely dispersed fissure defects Larger, isolated fissure defects