‫ﻋﻠﻤﯽ‬ ‫ﻣﺠﻠﻪ‬-‫ﭘﮋوﻫﺸﯽ‬
»‫ﻣــﺪرس‬ ‫ﻋﻤـﺮان‬«
‫دوره‬‫دوازدﻫﻢ‬‫ﺷﻤﺎره‬ ،4،‫زﻣﺴﺘﺎن‬1391
‫ﺗﺤﻘﯿﻘﺎﺗﯽ‬ ‫ﯾﺎدداﺷﺖ‬:
‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫و‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﺮرﺳﯽ‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬
‫ﺳﺒﮏ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫داﻧﻪ‬
‫ﺧﺎﻧﺰادي‬ ‫ﻣﺼﻄﻔﯽ‬1*
‫ﻋﻠﯿﺮﺿﺎ‬ ،‫ﭼﺎﻟﻪ‬‫ﮐﺎﯾﯽ‬2
1-‫اﯾﺮان‬ ‫ﺻﻨﻌﺖ‬ ‫و‬ ‫ﻋﻠﻢ‬ ‫داﻧﺸﮕﺎه‬ ،‫ﻋﻤﺮان‬ ‫داﻧﺸﮑﺪه‬ ،‫اﺳﺘﺎدﯾﺎر‬
2-‫اﯾﺮان‬ ‫ﺻﻨﻌﺖ‬ ‫و‬ ‫ﻋﻠﻢ‬ ‫داﻧﺸﮕﺎه‬ ،‫ﻋﻤﺮان‬ ‫داﻧﺸﮑﺪه‬ ،‫ارﺷﺪ‬ ‫ﮐﺎرﺷﻨﺎس‬
khanzadi@iust.ac.ir
‫درﯾﺎﻓﺖ‬ ‫ﺗﺎرﯾﺦ‬:07/10/1390‫ﭘﺬﯾﺮش‬ ‫ﺗﺎرﯾﺦ‬:20/12/1390
‫ﭼﮑﯿﺪه‬-‫ا‬ ‫در‬‫ﯾ‬‫ﻦ‬‫ﭘﮋوﻫﺶ‬‫ﺳﻨﮕﺪاﻧﻪ‬ ‫از‬ ‫اﺳﺘﻔﺎده‬ ‫اﻣﮑﺎن‬‫ﻫﺎ‬‫ي‬‫اﺳﮑﻮر‬‫ﯾ‬‫ﺎ‬‫ﻟ‬ ‫و‬‫ﯿ‬‫ﮑﺎ‬‫ي‬‫ﺑ‬ ‫ﮐﺸﻮر‬ ‫در‬ ‫ﻣﻮﺟﻮد‬‫ﺮاي‬‫ﺗﻮﻟ‬‫ﯿ‬‫ﺪ‬‫ﺳـﺒﮏ‬ ‫ﺑـﺘﻦ‬‫ﭘﺮﻣﻘﺎوﻣـﺖ‬ ‫داﻧـﻪ‬
‫ﺑﺮرﺳ‬‫ﯽ‬‫اﺳﺖ‬ ‫ﺷﺪه‬.‫ﻃﺮح‬ ‫ﺑﺮاﺳﺎس‬‫ﻫﺎ‬‫ي‬‫ﮔﻮﻧﺎﮔﻮن‬‫اﺧﺘﻼط‬‫و‬‫روش‬‫ﻫﺎ‬‫ي‬‫ﺗﻮﻟ‬ ،‫ﻣﺮﺳﻮم‬‫ﯿ‬‫ﺪ‬‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬‫داﻧـﻪ‬‫ا‬‫ي‬‫ﻓﺸـﺎر‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﺑـﺎ‬‫ي‬28‫روزه‬‫ي‬
‫ﺑ‬‫ﯿ‬‫ﺸﺘﺮ‬‫از‬40‫آن‬ ‫ﺑﺘﻮان‬ ‫ﮐﻪ‬ ‫ﻣﮕﺎﭘﺎﺳﮑﺎل‬‫ﺑ‬ ‫در‬ ‫را‬‫ﺘﻦ‬‫ﺑ‬ ‫ﻣﺴﻠﺢ‬‫ﻪ‬‫ﮐ‬‫ﺷﺪ‬ ‫ﻣﻤﮑﻦ‬ ،‫ﺑﺮد‬ ‫ﺎر‬.‫ﺑ‬‫ﺮاي‬‫ﺑﺮرﺳ‬‫ﯽ‬‫ﻣﮑـﺎﻧ‬ ‫ﻣﺸﺨﺼﺎت‬‫ﯿ‬‫ﮑ‬‫ﯽ‬‫ﮐﻮﺗـﺎه‬‫ا‬ ‫ﻣـﺪت‬‫ﯾـ‬‫ﻦ‬‫ﺑـﺘﻦ‬،
‫آزﻣﺎ‬‫ﯾ‬‫ﺶ‬‫ﻫﺎ‬‫ي‬‫ﻣﺨﺘﻠﻔ‬‫ﯽ‬‫ﻓﺸﺎر‬ ‫ﻣﻘﺎوﻣﺖ‬ ،‫ﺑﺘﻦ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﭼﻮن‬‫ي‬،‫اﻻﺳﺘ‬ ‫ﻣﺪول‬‫ﯿ‬‫ﺴ‬‫ﯿ‬‫ﺘﻪ‬‫اﺳﺘﺎﺗ‬‫ﯿ‬‫ﮑ‬‫ﯽ‬‫ﺿﺮ‬ ‫و‬‫ﯾ‬‫ﺐ‬‫ﺷﺪ‬ ‫اﻧﺠﺎم‬ ‫ﭘﻮاﺳﻮن‬‫؛‬‫رواﺑﻄ‬‫ﯽ‬‫ﻧ‬‫ﯿـ‬‫ﺰ‬
‫ﺑﺮاي‬‫ﭘ‬‫ﯿ‬‫ﺶ‬‫ﺑ‬‫ﯿ‬‫ﻨ‬‫ﯽ‬‫اﻻﺳﺘ‬ ‫ﻣﺪول‬‫ﯿ‬‫ﺴ‬‫ﯿ‬‫ﺘﻪ‬‫اﺳﺘﺎﺗ‬‫ﯿ‬‫ﮑ‬‫ﯽ‬‫ا‬‫ﯾ‬‫ﻦ‬‫ﺑﺘﻦ‬‫ﻫﺎ‬‫ﻣﺨﺼﻮﺻﺸﺎن‬ ‫وزن‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﺮاﺳﺎس‬‫ﺳﻦ‬ ‫در‬28‫اﺳـﺖ‬ ‫ﺷـﺪه‬ ‫اراﺋﻪ‬ ‫روز‬.
‫ﻣﺸﺨﺺ‬‫ﺷ‬‫ﺑ‬ ‫ﺑﺘﻦ‬ ‫وزن‬ ‫اﻓﺰاﯾﺶ‬ ‫ﺑﺎ‬ ‫ﮐﻪ‬ ‫ﺪ‬‫ﺎ‬‫داﻧﻪ‬ ‫ﺑﺎﻓﺖ‬ ‫در‬ ‫ﺗﻐﯿﯿﺮ‬‫ﺑـﺘﻦ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ،‫ﺑﻨﺪي‬‫آزﻣـﺎﯾﺶ‬ ‫ﻫـﺎي‬،‫ﺷـﺪه‬‫اﻓـﺰاﯾﺶ‬
‫اﺳﺖ‬ ‫ﯾﺎﻓﺘﻪ‬.‫ﺑﺘﻦ‬ ‫اﯾﻦ‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﻬﺒﻮد‬ ‫در‬ ‫ﻧﯿﺰ‬ ‫ﺳﯿﻠﯿﺴﯽ‬ ‫دوده‬ ‫از‬ ‫اﺳﺘﻔﺎده‬‫ﺑﻮ‬ ‫ﻣﺆﺛﺮ‬ ‫ﻫﺎ‬‫اﺳﺖ‬ ‫ده‬.‫ﻣﯽ‬ ‫ﻧﺸﺎن‬ ‫ﻧﺘﺎﯾﺞ‬‫ﻟﯿﮑـﺎ‬ ‫و‬ ‫اﺳـﮑﻮرﯾﺎ‬ ‫ﮐﻪ‬ ‫دﻫﻨﺪ‬
‫ﻧﻤﻮﻧﻪ‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﻬﺒﻮد‬ ‫در‬‫ﺑﻮده‬ ‫ﻣﺆﺛﺮ‬ ‫ﻫﺎ‬‫ﻣﻨﺎﺳـﺐ‬ ‫ﻧﺘﺎﯾﺞ‬ ‫ﺑﻪ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﮐﻪ‬‫اﺳـﺖ‬ ‫رﺳـﯿﺪه‬ ‫ﺗـﺮي‬.‫ﺗـﻨﺶ‬ ‫ﻣﻨﺤﻨـﯽ‬-‫ﺑـﺘﻦ‬ ‫ﮐـﺮﻧﺶ‬‫ﻫـﺎي‬
‫ﻣﻄﺎﻟﻌﻪ‬‫ﺗﻮﺻﯿﻪ‬ ‫و‬ ‫ﺷﺪ‬ ‫ﺑﺮرﺳﯽ‬ ‫ﺷﺪه‬‫ﻣﻨﺤﻨﯽ‬ ‫اﯾﻦ‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﺮاي‬ ‫ﻫﺎﯾﯽ‬‫ﺷﺪ‬ ‫اراﺋﻪ‬ ‫ﻫﺎ‬.‫ﻣﻨﺤﻨﯽ‬ ،‫ﻧﺘﺎﯾﺞ‬ ‫اﺳﺎس‬ ‫ﺑﺮ‬‫ﺷﺎﺧﻪ‬ ‫در‬ ‫ﻫﺎ‬‫ﻫـﺎي‬‫ﻧﺰوﻟـﯽ‬ ‫و‬ ‫ﺻـﻌﻮدي‬
‫ﺑﻮدﻧﺪ‬ ‫ﺧﻄﯽ‬ ً‫ﺎ‬‫ﺗﻘﺮﯾﺒ‬.
‫واژﮔﺎن‬‫ﮐﻠﯿﺪ‬‫ي‬:‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ،‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ،‫اﺳﮑﻮرﯾﺎ‬ ،‫ﻟﯿﮑﺎ‬ ،‫داﻧﻪ‬-‫ﮐﺮﻧﺶ‬
1-‫ﻣﻘﺪﻣﻪ‬
‫ﺑـﺎ‬ ‫ﺳﺒﮏ‬ ‫ﻣﺼﺎﻟﺢ‬ ‫ﺑﺮاي‬ ‫ﺗﻘﺎﺿﺎ‬ ‫و‬ ‫ﯾﺎﻓﺘﻪ‬ ‫اﻓﺰاﯾﺶ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﺗﻮﻟﯿﺪ‬
‫ﻫـﻢ‬ ‫ﺳـﺎز‬ ‫و‬ ‫ﺳـﺎﺧﺖ‬ ‫ﺑـﺮاي‬ ‫ﻗﺒـﻮل‬ ‫ﻗﺎﺑﻞ‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬
‫ﻣﯽ‬ ‫اﻓﺰاﯾﺶ‬‫ﯾﺎﺑﺪ‬.‫ﺑـﺘﻦ‬ ‫از‬ ،‫ﺑـﺘﻦ‬ ‫ﻣﺨﺘﻠﻒ‬ ‫اﻧﻮاع‬ ‫ﺷﺎﻣﻞ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬
‫ﮐﻢ‬‫ﺑﻠﻮك‬ ‫ﺗﻮﻟﯿﺪ‬ ‫در‬ ‫ﺑﯿﺸﺘﺮ‬ ‫ﮐﻪ‬ ‫ﻣﻘﺎوﻣﺖ‬‫ﻏﯿﺮﺳﺎزه‬ ‫ﻫﺎي‬‫ﺑـﻪ‬ ‫اي‬‫ﮐـﺎر‬
‫ﻣﯽ‬‫ﺑﺘﻦ‬ ‫ﺗﺎ‬ ‫رود‬‫ﺳﺎزه‬ ‫ﻫﺎي‬‫از‬ ‫ﺑـﯿﺶ‬ ‫ﻓﺸـﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﺎ‬ ‫اي‬100
‫ﻣﯽ‬ ‫ﻣﮕﺎﭘﺎﺳﮑﺎل‬‫ﺷﻮد‬.‫ﺑﺴﯿﺎري‬ ‫ﻣﺤﻘﻘﯿﻦ‬]3-1[‫ﺗﺤﻘﯿﻘﺎﺗﺸﺎن‬ ‫در‬
‫آورده‬‫ﺳﺒﮏ‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫ﻫﻮاي‬ ‫ﺣﻔﺮات‬ ‫ﺧﺎﻃﺮ‬ ‫ﺑﻪ‬ ‫ﮐﻪ‬ ‫اﻧﺪ‬‫داﻧﻪ‬،‫ﻫـﺎ‬
‫ﻣﻘﺎوﻣـﺖ‬ ،‫وزن‬ ‫ﺑـﻪ‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﺑـﺎﻻي‬ ‫ﻧﺴـﺒﺖ‬ ‫داراي‬ ‫ﺑـﺘﻦ‬ ‫اﯾﻦ‬
‫وﯾﮋﮔﯽ‬ ‫و‬ ‫ﭘﺎﯾﯿﻦ‬ ‫ﺣﺮارﺗﯽ‬ ‫اﻧﺒﺴﺎط‬ ‫ﺿﺮﯾﺐ‬ ،‫ﻣﻨﺎﺳﺐ‬ ‫ﮐﺸﺸﯽ‬‫ﻫﺎي‬
‫دارد‬ ‫را‬ ‫ﺻﺪا‬ ‫و‬ ‫ﮔﺮﻣﺎ‬ ‫ﻣﻘﺎﺑﻞ‬ ‫در‬ ‫ﺑﻮدن‬ ‫ﻋﺎﯾﻖ‬ ‫ﺑﺮﺗﺮ‬.‫ﺑﺮ‬ ‫اﻓﺰون‬،‫اﯾﻦ‬
‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫در‬‫ﺳـﺎزه‬ ‫اﻋﻀﺎي‬ ‫ﻋﺮﺿﯽ‬ ‫ﻣﻘﻄﻊ‬ ،‫ﺗﺮ‬‫ﮐﻮﭼـﮏ‬ ‫اي‬‫ﺗـﺮ‬
‫ﻣﯽ‬‫اﻗﺘﺼﺎدي‬ ‫اﺟﺮا‬ ‫و‬ ‫ﺷﻮد‬‫ﺷﺪ‬ ‫ﺧﻮاﻫﺪ‬ ‫ﺗﺮ‬.
‫ﺳـﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﻫﺮ‬ ‫ﺗﻮﻟﯿﺪ‬‫ﺑـﻮدن‬ ‫دﺳـﺘﺮس‬ ‫در‬ ‫ﺑـﻪ‬ ً‫ﻼ‬‫ﮐـﺎﻣ‬ ‫داﻧـﻪ‬
‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫و‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﺮرﺳﯽ‬-‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫داﻧﻪ‬‫ﭼﺎﻟﻪ‬ ‫ﻋﻠﯿﺮﺿﺎ‬ ‫و‬ ‫ﺧﺎﻧﺰادي‬ ‫ﻣﺼﻄﻔﯽ‬‫ﮐﺎﯾﯽ‬
80
‫ﺳﺒﮏ‬‫داﻧـﻪ‬‫اﺳـﺖ‬ ‫ﻣـﺮﺗﺒﻂ‬ ‫ﻫـﺎ‬]4.[‫ﻣﺤﻘﻘـﯿﻦ‬ ‫ﺑﺮﺧـﯽ‬]4،3[‫در‬
‫ﺑﺘﻦ‬ ‫روي‬ ‫ﺗﺤﻘﯿﻘﺎﺗﺸﺎن‬‫ﺳﺒﮏ‬ ‫ﻫﺎي‬‫ﺳـﺒﮏ‬ ‫ﺣﺎوي‬ ‫داﻧﻪ‬‫داﻧـﻪ‬‫ﻫـﺎي‬
‫ﺗﻮف‬ ‫ﭼﻮن‬ ‫ﻃﺒﯿﻌﯽ‬1
‫ﭘﺮﻟﯿﺖ‬ ‫و‬2
‫ﺳـﺒﮏ‬ ‫ﯾﺎ‬‫داﻧـﻪ‬‫ﻣﺼـﻨﻮﻋﯽ‬ ‫ﻫـﺎي‬
‫ﻣﻨﺒﺴﻂ‬ ‫رس‬ ‫ﭼﻮن‬‫ﺷﻞ‬ ‫ﯾﺎ‬ ‫ﺷﺪه‬3
‫ﮐﺮده‬ ‫ﻣﻄﺎﻟﻌﻪ‬‫اﻧﺪ‬.‫آن‬‫اﯾـﻦ‬ ‫ﺑـﻪ‬ ‫ﻫﺎ‬
‫رﺳﯿﺪه‬ ‫ﻧﺘﯿﺠﻪ‬‫اﻓﺰودﻧـﯽ‬ ‫ﮐـﻪ‬ ‫اﻧـﺪ‬،‫ﺑـﺎدي‬ ‫ﺧﺎﮐﺴـﺘﺮ‬ ‫ﻣﺎﻧﻨـﺪ‬ ‫ﻫـﺎﯾﯽ‬
‫ﭘﻮزوﻻن‬ ‫و‬ ‫ﻣﯿﮑﺮوﺳﯿﻠﯿﺲ‬‫ﺳـﺒﺐ‬ ،‫ﺳـﺒﮏ‬ ‫ﺑـﺘﻦ‬ ‫در‬ ‫ﻃﺒﯿﻌﯽ‬ ‫ﻫﺎي‬
‫ـﯽ‬‫ـ‬‫ﻣ‬ ‫ـﺘﻦ‬‫ـ‬‫ﺑ‬ ‫در‬ ‫ـﯽ‬‫ـ‬‫ﻣﺨﺘﻠﻔ‬ ‫ـﺎت‬‫ـ‬‫ﻣﺸﺨﺼ‬ ‫ـﻮد‬‫ـ‬‫ﺑﻬﺒ‬‫ـﻪ‬‫ـ‬‫ﮐ‬ ‫ـﺮا‬‫ـ‬‫ﭼ‬ ‫ـﻮد؛‬‫ـ‬‫ﺷ‬
‫واﮐﻨﺶ‬‫ﻣﺸﺨﺼـﺎ‬ ‫ﺑﻬﺒـﻮد‬ ‫ﺑﻪ‬ ‫ﻣﻨﺠﺮ‬ ‫ﭘﻮزوﻻﻧﯽ‬ ‫ﻫﺎي‬‫ﻣﮑـﺎﻧﯿﮑﯽ‬ ‫ت‬
‫ﻣﯽ‬‫ﺷﻮد‬]5[.‫ﺳـﺎزه‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫در‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬،‫اي‬21‫ﺗـﺎ‬
28‫اﺳﺖ‬ ‫ﻣﮕﺎﭘﺎﺳﮑﺎل‬]6[‫ﻣـﻮاد‬ ‫ﺑـﻪ‬ ‫آب‬ ‫ﻧﺴـﺒﺖ‬ ‫ﮐﺎﻫﺶ‬ ‫ﺑﺎ‬ ‫ﮐﻪ‬
،‫ذرات‬ ‫ـﺪازه‬‫ـ‬‫اﻧ‬ ‫ـﯿﻨﮥ‬‫ـ‬‫ﺑﯿﺸ‬ ‫ـﺎﻫﺶ‬‫ـ‬‫ﮐ‬ ،‫ـﯿﻤﺎن‬‫ـ‬‫ﺳ‬ ‫ـﺰاﯾﺶ‬‫ـ‬‫اﻓ‬ ،‫ـﺒﻨﺪه‬‫ـ‬‫ﭼﺴ‬
‫ﺳـﺒﮏ‬ ‫ﻣﺎﺳﻪ‬ ‫ﺟﺎﯾﮕﺰﯾﻨﯽ‬‫از‬ ‫اﺳـﺘﻔﺎده‬ ‫و‬ ‫ﻃﺒﯿﻌـﯽ‬ ‫ﻣﺎﺳـﻪ‬ ‫ﺑـﺎ‬ ‫داﻧـﻪ‬
‫اﻓﺰودﻧﯽ‬‫ﻣﯽ‬ ‫اﻓﺰاﯾﺶ‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫اﯾﻦ‬ ‫ﻫﺎ‬‫ﯾﺎﺑﺪ‬.
‫ﺿﻌﯿﻒ‬‫ﺟﺰ‬ ‫ﺗﺮﯾﻦ‬‫ﻣﻨﻄﻘـﻪ‬ ‫ﯾـﺎ‬ ‫ﺳـﯿﻤﺎن‬ ‫ﻣﺎﺗﺮﯾﺲ‬ ،‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ء‬
‫ﺗﻤﺎﺳﯽ‬4
‫ﺳـﺒﮏ‬ ‫ﺑﻠﮑـﻪ‬ ،‫ﻧﯿﺴـﺖ‬‫اﺳـﺖ‬ ‫داﻧـﻪ‬.‫دﻟﯿـﻞ‬ ‫ﻫﻤـﯿﻦ‬ ‫ﺑـﻪ‬
‫ﺳﯿﻤﺎن‬ ‫ﻣﺎﺗﺮﯾﺲ‬ ‫ﮐﯿﻔﯿﺖ‬ ‫ﺑﺎ‬ ‫ﺗﻨﻬﺎ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬
‫ﻧﻤــﯽ‬ ‫ﺳــﻨﺠﯿﺪه‬ ‫آن‬‫ﺳــﺒﮏ‬ ‫ﻣﺸﺨﺼــﺎت‬ ‫و‬ ‫ﺷــﻮد‬‫ﺣﺠــﻢ‬ ‫داﻧــﻪ‬
‫ﺳﺒﮏ‬‫داﻧﻪ‬‫ﺳﺒﮏ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫و‬ ‫ﺑﺘﻦ‬ ‫در‬ ‫ﻫﺎ‬‫ﻣـﻮرد‬ ‫اﯾﻦ‬ ‫در‬ ‫ﻧﯿﺰ‬ ‫داﻧﻪ‬
‫ﻣﻮﺛﺮﻧﺪ‬]7،3[.
‫ﺟﻮرو‬ ‫و‬ ‫ژاﻧﮓ‬]8[‫ﺗﺎﺛﯿﺮ‬‫ﻣﻘﺎوﻣـﺖ‬ ‫ﺑـﺮ‬ ‫ﺳـﺒﮏ‬ ‫ﺑـﺘﻦ‬ ‫ﭼﮕﺎﻟﯽ‬
‫ﺑﺮرﺳﯽ‬ ‫را‬ ‫ﭘﺮﻣﻘﺎوﻣﺖ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮔﺴﯿﺨﺘﮕﯽ‬ ‫ﺳﺎزوﮐﺎر‬ ‫و‬ ‫ﻓﺸﺎري‬
‫ﮐﺮده‬‫اﻧﺪ‬.‫ﺳـﺒﮏ‬ ‫ﮐـﻢ‬ ‫ﺣﺠـﻢ‬ ‫اﻫﻤﯿـﺖ‬ ‫ﺑﺴﯿﺎري‬ ‫ﻣﺤﻘﻘﯿﻦ‬‫در‬ ‫داﻧـﻪ‬
‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬‫ﺑـﺎ‬ ‫ﺗﻨﻬـﺎ‬ ‫را‬ ‫داﻧـﻪ‬
‫ﭼﮕﺎﻟﯽ‬‫ﻣﯽ‬ ‫ﺷﺎن‬‫ﻣﮑـﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼـﺎت‬ ‫ﺳﻨﺠﺶ‬ ‫ﮐﻪ‬ ‫ﭼﺮا‬ ‫ﺳﻨﺠﻨﺪ؛‬
‫ﺳﺒﮏ‬‫داﻧﻪ‬‫اﺳﺖ‬ ‫دﺷﻮار‬ ‫ﻫﺎ‬]3‫و‬9[.‫و‬‫ﺑﻨﺘـﻮر‬ ‫و‬ ‫اﺳﺮﻣﻦ‬]10[‫ﻧﺸـﺎن‬
‫داده‬‫ﺳـﻨﮕﺪاﻧﻪ‬ ‫ﯾﮑﺴﺎن‬ ‫ﭼﮕﺎﻟﯽ‬ ‫ﮐﻪ‬ ‫اﻧﺪ‬‫اﯾﺠـﺎد‬ ‫ﺳـﺒﺐ‬ ً‫ﻻ‬‫ﻣﻌﻤـﻮ‬ ‫ﻫـﺎ‬
‫ﻧﻤﯽ‬ ‫ﺑﺘﻦ‬ ‫در‬ ‫ﯾﮑﺴﺎن‬ ‫ﻣﻘﺎوﻣﺖ‬‫ﺷﻮد‬.
‫روش‬ ‫ﺑﺎ‬ ‫را‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬‫ﻣﯽ‬ ‫ﺗﻮﻟﯿﺪ‬ ‫ﻣﺨﺘﻠﻔﯽ‬ ‫ﻫﺎي‬‫ﮐﻨﻨـﺪ‬.‫ﺑـﺮاي‬
1- tuff
2- perlite
3- shale
4- interfacial transition zone
‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫داﺷﺘﻦ‬‫ﺳﺎزه‬ ‫داﻧﻪ‬‫ﺳﺒﮏ‬ ،‫ﭘﺮﻣﻘﺎوﻣﺖ‬ ‫و‬ ‫اي‬‫داﻧـﻪ‬‫ﺑـﻪ‬ ‫ﻫـﺎ‬
‫ﺳﻨﮓ‬ ‫از‬ ‫ﺑﺨﺸﯽ‬ ‫ﺟﺎﯾﮕﺰﯾﻦ‬ ‫ﻋﻨﻮان‬‫داﻧﻪ‬‫ﻫﻤـ‬ ‫ﯾﺎ‬ ‫ﻣﻌﻤﻮﻟﯽ‬ ‫ﻫﺎي‬‫آن‬ ‫ﻪ‬
‫ﻣﯽ‬ ‫ﮐﺎر‬ ‫ﺑﻪ‬‫رود‬.‫ﺳﺒﮏ‬ ‫ﮐﻠﯽ‬ ‫ﻃﻮر‬ ‫ﺑﻪ‬‫داﻧﻪ‬‫و‬ ‫ﻃﺒﯿﻌـﯽ‬ ‫ﻧﻮع‬ ‫دو‬ ‫ﺑﻪ‬ ‫ﻫﺎ‬
‫ﻣـﯽ‬ ‫ﺗﻘﺴـﯿﻢ‬ ‫ﻣﺼﻨﻮﻋﯽ‬‫ﺷـﻮﻧﺪ‬.‫ﺳـﺒﮏ‬‫از‬ ‫ﭘـﺲ‬ ‫را‬ ‫ﻃﺒﯿﻌـﯽ‬ ‫داﻧـﻪ‬
‫داﻧﻪ‬ ً‫ﺎ‬‫ﻣﺴﺘﻘﯿﻤ‬ ،‫ﻣﻌﺪن‬ ‫از‬ ‫اﺳﺘﺨﺮاج‬‫ﺑـﻪ‬ ‫ﺑﺘﻦ‬ ‫در‬ ‫و‬ ‫ﮐﺮده‬ ‫ﺑﻨﺪي‬‫ﮐـﺎر‬
‫ﻣﯽ‬‫ﺑﺮﻧﺪ‬.‫راﯾﺞ‬ ‫از‬ ‫ﯾﮑﯽ‬‫ﺳﺒﮏ‬ ‫ﺗﺮﯾﻦ‬‫داﻧﻪ‬‫در‬ ‫ﻣﻮﺟـﻮد‬ ‫ﻃﺒﯿﻌﯽ‬ ‫ﻫﺎي‬
‫اﯾﺮان‬"‫اﺳﮑﻮرﯾﺎ‬"‫ﺑﺎ‬ ‫ﻋﺎم‬ ‫زﺑﺎن‬ ‫در‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬‫ﻋﻨﻮان‬"‫ﭘـﺎ‬ ‫ﺳﻨﮓ‬"
‫ﻣﯽ‬ ‫ﺷﻨﺎﺧﺘﻪ‬‫ﺷﻮد‬.‫ﭘﻮﮐﻪ‬ ‫ﺟﺰء‬ ‫و‬ ‫دارد‬ ‫آذرﯾﻦ‬ ‫ﻣﻨﺸﺄ‬ ‫اﺳﮑﻮرﯾﺎ‬‫ﻫﺎي‬
‫اﺳﺖ‬ ‫ﻣﻌﺪﻧﯽ‬.‫ﮐﻮه‬ ‫دﻫﺎﻧﻪ‬ ‫در‬ ‫ﺑﯿﺸﺘﺮ‬ ‫ﺳﻨﮓ‬ ‫اﯾﻦ‬‫آﺗﺸﻔﺸـﺎﻧﯽ‬ ‫ﻫﺎي‬
‫ﮔﺪازه‬ ‫از‬ ‫و‬‫دارﻧـﺪ‬ ‫ﮐﻤـﯽ‬ ‫ﺳـﯿﻠﯿﺲ‬ ‫ﮐـﻪ‬ ‫ﻣﺬاﺑﯽ‬ ‫ﻫﺎي‬)‫ﺑﺎزاﻟـﺖ‬5
(
‫ﻣﯽ‬ ‫اﯾﺠﺎد‬‫ﺷﻮد‬.‫ﻣﯽ‬ ‫و‬ ‫اﺳﺖ‬ ‫ﺗﯿﺮه‬ ‫آن‬ ‫رﻧﮓ‬‫رﻧـﮓ‬ ‫ﺑـﻪ‬ ‫ﺗﻮاﻧﺪ‬‫ﻫـﺎي‬
‫ﻗﻬﻮه‬‫ﺧﺎﮐﺴـﺘﺮ‬ ،‫ﻗﺮﻣـﺰ‬ ،‫ﻗﺮﻣﺰ‬ ‫ﺑﻪ‬ ‫ﻣﺎﯾﻞ‬ ‫اي‬‫ﺑﺎﺷـﺪ‬ ‫ﺳـﯿﺎه‬ ‫ﯾـﺎ‬ ‫و‬ ‫ي‬.
‫ﺳﻨﮓ‬ ‫اﯾﻦ‬ ‫ﺑﯿﺸﺘﺮ‬‫دارﻧﺪ‬ ‫ﯾﮏ‬ ‫از‬ ‫ﺑﯿﺸﺘﺮ‬ ‫ﻣﺨﺼﻮﺻﯽ‬ ‫وزن‬ ‫ﻫﺎ‬]11[.
‫ﺳـﺎزه‬ ‫اﻋﻀـﺎي‬ ‫ﺗﻮﻟﯿـﺪ‬ ‫در‬ ‫ﭼﻨﺪاﻧﯽ‬ ‫ﮐﺎرﺑﺮد‬ ‫ﻣﺎده‬ ‫اﯾﻦ‬ ‫ﺗﺎﮐﻨﻮن‬‫اي‬
‫اﺳـﮑﻮرﯾﺎ‬ ‫از‬ ‫اﺳﺘﻔﺎده‬ ‫ﻣﻮرد‬ ‫در‬ ‫ﮐﻤﯽ‬ ‫ﺗﺤﻘﯿﻘﺎت‬ ‫و‬ ‫اﺳﺖ‬ ‫ﻧﺪاﺷﺘﻪ‬
‫اﺳـﺖ‬ ‫ﺷﺪه‬ ‫اﻧﺠﺎم‬ ‫ﭘﺮﻣﻘﺎوﻣﺖ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫در‬.‫اﺳـﮑﻮرﯾﺎ‬ ‫ﻣﻌـﺎدن‬
‫ﺗﻮﺟﻪ‬ ‫ﻗﺎﺑﻞ‬ ‫ﮐﺸﻮر‬ ‫ﻏﺮب‬ ‫ﺷﻤﺎل‬ ‫و‬ ‫ﻏﺮب‬ ‫در‬‫اﺳﺖ‬.
‫ﺳﺒﮏ‬ ‫ﺟﻤﻠﻪ‬ ‫از‬‫داﻧﻪ‬‫ﻣﻨﺒﺴﻂ‬ ‫رس‬ ،‫ﻣﺼﻨﻮﻋﯽ‬ ‫ﻫﺎي‬‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫ﺷﺪه‬
‫ﻣـﯽ‬ ‫ﻧﺎﻣﯿـﺪه‬ ‫ﻟﯿﮑﺎ‬ ‫اﻏﻠﺐ‬‫ﺷـﻮد‬.،‫ﻟﯿﮑـﺎ‬ ‫ﺑـﺎ‬ ‫ﻣﺨﺘﻠـﻒ‬ ‫ﮐﺸـﻮرﻫﺎي‬ ‫در‬
‫ﺑﺘﻦ‬‫ﺗﻤﺎم‬ ‫ﻫﺎي‬‫ﺳﺒﮏ‬‫ﻧﯿﻤﻪ‬ ‫ﯾﺎ‬ ‫داﻧﻪ‬‫ﺳﺒﮏ‬‫ﺳﺎزه‬ ‫داﻧﻪ‬‫ﻣﯽ‬ ‫را‬ ‫اي‬‫ﺳـﺎزﻧﺪ‬.‫در‬
‫ﻣﯽ‬ ‫ﺗﻮﻟﯿﺪ‬ ‫ﺳﺒﮑﯽ‬ ‫ﻟﯿﮑﺎي‬ ‫ﻣﺎ‬ ‫ﮐﺸﻮر‬‫ﺳـﺎﺧﺖ‬ ‫ﺑـﺮاي‬ ً‫ﻻ‬‫ﻣﻌﻤﻮ‬ ‫ﮐﻪ‬ ‫ﺷﻮد‬
‫ﺑﺘﻦ‬‫ﺷﯿﺐ‬ ،‫ﭘﺮﮐﻨﻨﺪه‬ ‫ﻫﺎي‬‫ﺑﺎم‬ ‫ﺑﻨﺪي‬‫و‬ ‫ﻫﺎ‬‫ﺑﻠـﻮك‬ ‫ﺳﺎﺧﺖ‬‫ﺳـﺒﮏ‬ ‫ﻫـﺎي‬
‫ـﺎزه‬‫ـ‬‫ﺳ‬ ‫ﻧﯿﻤـﻪ‬ ‫ـﺎرﺑﺮد‬‫ـ‬‫ﮐ‬ ‫ﮐـﻪ‬‫ﻣـﯽ‬ ‫ـﺘﻔﺎده‬‫ـ‬‫اﺳ‬ ،‫دارد‬ ‫اي‬‫ـﻮد‬‫ـ‬‫ﺷ‬.‫ـﺎت‬‫ـ‬‫ﺗﺤﻘﯿﻘ‬
‫ﺑﺘﻦ‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺗﻌﯿﯿﻦ‬ ‫در‬ ‫ﺳﻌﯽ‬ ‫ﻣﺨﺘﻠﻔﯽ‬‫ﺑﺎ‬ ‫ﺷﺪه‬ ‫ﺳﺎﺧﺘﻪ‬ ‫ﻫﺎي‬
‫اﺳﺖ‬ ‫داﺷﺘﻪ‬ ‫ﻣﺨﺘﻠﻒ‬ ‫ﺷﺮاﯾﻂ‬ ‫در‬ ‫را‬ ‫اﯾﺮان‬ ‫ﻟﯿﮑﺎي‬.
‫ﻣﺸﺨﺺ‬‫ﺗـﻨﺶ‬ ‫ﻣﻨﺤﻨـﯽ‬ ‫ﺗﺨﻤـﯿﻦ‬ ‫ﺑﺮاي‬ ‫ﮐﻪ‬ ‫رواﺑﻄﯽ‬ ‫ﺗﺮﯾﻦ‬-
‫ﺷـﮑﻞ‬ ‫در‬ ‫ﺷﺪه‬ ‫اراﺋﻪ‬ ‫ﮐﺮﻧﺶ‬)1(‫اﺳـﺖ‬ ‫ﺷـﺪه‬ ‫آورده‬.‫ﻣﻨﺤﻨـﯽ‬
‫ﺗ‬‫ﻮدﭼﯿﻨﯽ‬‫ﺗﺤﻠﯿﻠـﯽ‬ ‫ﻣﻄﺎﻟﻌـﺎت‬ ‫ﺑـﺮاي‬ ،‫آن‬ ‫ﭘﯿﻮﺳـﺘﻪ‬ ‫ﺗﺎﺑﻊ‬ ‫دﻟﯿﻞ‬ ‫ﺑﻪ‬
‫اﺳﺖ‬ ‫ﻣﻨﺎﺳﺐ‬]12[.
5- basalt
‫ﺷﻤﺎره‬ ،‫دوازدﻫﻢ‬ ‫دوره‬4/‫زﻣﺴﺘﺎن‬1391
‫ﮐﻮﺗﺎه‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫از‬ ‫ﺑﺮﺧﯽ‬ ‫ﺗﻌﯿﯿﻦ‬ ،‫ﺑﻌﺪ‬ ‫ﻣﺮﺣﻠﻪ‬‫ﻣـﺪت‬
‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﮐﺸﺸﯽ‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻣﺎﻧﻨﺪ‬ ‫ﺑﺘﻦ‬ ‫اﯾﻦ‬
‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺑﺮرﺳﯽ‬ ‫و‬-‫اﺳﺖ‬ ‫آن‬ ‫ﮐﺮﻧﺶ‬.
‫آزﻣﺎﯾﺸﮕﺎﻫﯽ‬ ‫اﻃﻼﻋﺎت‬
‫ﻣﺼﺮﻓﯽ‬ ‫ﻣﺼﺎﻟﺢ‬
‫ـﻪ‬‫ـ‬‫ﻧﻤﻮﻧ‬ ‫ـﮥ‬‫ـ‬‫ﻫﻤ‬ ‫ﺳـﺎﺧﺖ‬ ‫در‬‫ـﻮع‬‫ـ‬‫ﻧ‬ ‫ـﯿﻤﺎن‬‫ـ‬‫ﺳ‬ ،‫ﻫـﺎ‬I‫ـﯽ‬‫ـ‬‫ﺳﯿﻠﯿﺴ‬ ‫دوده‬ ،
،‫ازﻧـﺎ‬ ‫در‬ ‫واﻗـﻊ‬ ‫اﯾـﺮان‬ ‫ﻓﺮوآﻟﯿـﺎژ‬ ‫ﺻـﻨﺎﯾﻊ‬ ‫ﺷﺮﮐﺖ‬ ‫در‬ ‫ﺗﻮﻟﯿﺪﺷﺪه‬
‫اﺳﺘﺨﺮاج‬ ‫اﺳﮑﻮرﯾﺎي‬ ‫و‬ ‫اﯾﺮاﻧﯽ‬ ‫داﻧﻪ‬‫ﻗـﺮوه‬ ‫از‬ ‫ﺷﺪه‬
12‫ﻣﯿﻠﯽ‬‫درﺷﺖ‬ ‫ﻋﻨﻮان‬ ‫ﺑﻪ‬ ‫ﻣﺘﺮ‬‫رﯾﺰداﻧـﻪ‬ ،‫داﻧﻪ‬
‫ـﯽ‬‫ـ‬‫اﻓﺰودﻧ‬ ‫ـﯿﻦ‬‫ـ‬‫ﻫﻤﭽﻨ‬ ‫و‬ ‫ـﺎك‬‫ـ‬‫ﻣﺘﻮﺳ‬ ‫ـﺮﮐﺖ‬‫ـ‬‫ﺷ‬ ‫ـﺪي‬‫ـ‬‫ﺗﻮﻟﯿ‬ ‫ـﻮﻟﯽ‬‫ـ‬‫ﻣﻌﻤ‬
‫ﻣﺤ‬ ،‫ﻧﻔﺘﺎﻟﯿﻦ‬ ‫ﭘﺎﯾﻪ‬ ‫ﺑﺮ‬ ‫ﮐﻨﻨﺪه‬‫ب‬ ‫ﺷـﺮﮐﺖ‬ ‫ﺼـﻮل‬.‫آ‬.‫اس‬.
‫ﺷﺪ‬ ‫اﺳﺘﻔﺎده‬ ‫اﯾﺮاﻧﯿﺎن‬ ‫اف‬.‫ﻧﻤﻮﻧﻪ‬ ‫ﻫﻤﮥ‬ ‫در‬‫ﺧﺸـﮏ‬ ‫رﯾﺰداﻧﻪ‬ ‫از‬ ‫ﻫﺎ‬
‫اﺳـﺖ‬ ‫ﺷـﺪه‬ ‫اﺳـﺘﻔﺎده‬ ‫ﺧﺸـﮏ‬ ‫ﺳـﺒﮏ‬ ‫داﻧﻪ‬.
‫ردﺷـﺪه‬ ‫درﺻـﺪ‬(‫ﺳـﺒﮏ‬‫داﻧـﻪ‬‫و‬ ‫ﻟﯿﮑـﺎ‬ ‫ﻫـﺎي‬
‫ـﺘﺎﻧﺪارد‬‫ـ‬‫اﺳ‬ ‫ـﺪوده‬‫ـ‬‫ﻣﺤ‬ ‫در‬ ‫ـﮑﻮرﯾﺎ‬‫ـ‬‫اﺳ‬ASTM C330]18[‫ـﺮار‬‫ـ‬‫ﻗ‬
‫ﻓﻮق‬ ‫و‬ ‫ﺳﯿﻤﺎن‬‫روان‬‫اﺳﺘﻔﺎده‬ ‫ﮐﻨﻨﺪه‬‫ﻧ‬ ‫ﺷﺪه‬‫ﺗﺮﺗﯿـﺐ‬ ‫ﺑـﻪ‬ ‫ﯿـﺰ‬
ASTM C]19[‫و‬ASTM C494]20[‫ـﻮده‬‫ـ‬‫ﺑ‬
‫اﻧﺒﻮﻫﯽ‬ ‫ﺧﺸﮏ‬ ‫ﻓﻀﺎﯾﯽ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬(3Kg/m)‫ﺑﺮاي‬
‫ﺗﺮﺗﯿـﺐ‬ ‫ﺑـﻪ‬ ‫اﺳـﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬430‫و‬702‫ﻣﺨﺼـﻮص‬ ‫وزن‬ ‫و‬
‫ﻣﯿﻠـﻪ‬ ‫ﺑﺎ‬ ‫ﻣﺘﺮاﮐﻢ‬ ‫ﺧﺸﮏ‬ ‫ﻓﻀﺎﯾﯽ‬(3Kg/m)‫وزن‬‫ﻫـﺎ‬507‫و‬783
‫اﻧﺒﻮﻫﯽ‬ ‫ﺧﺸﮏ‬ ‫ﻓﻀﺎﯾﯽ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﻣﯿﺰان‬ ‫ﺑﯿﺸﺘﺮﯾﻦ‬
‫اﺳـﺘﺎﻧﺪارد‬ ‫ﻃﺒـﻖ‬ ‫ﺳـﺒﮏ‬ ‫ﻫﺎي‬ASTM C330،
‫اﺳﺖ‬ ‫ﺷﺪه‬ ‫ﻗﯿﺪ‬.‫آب‬ ‫ﺟﺬب‬24‫داﻧﻪ‬ ‫ﺳﺎﻋﺘﻪ‬‫ﻫـﺎي‬
‫ﺗﺮﺗﯿﺐ‬ ‫ﺑﻪ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬8‫و‬5‫اﺳﺖ‬ ‫ﻣﯽ‬ ‫درﺻﺪ‬.
‫ﻣﺨﻠﻮط‬ ‫اﻧﺘﺨﺎب‬ ‫اﺻﻮل‬‫ﻧﺴﺒﺖ‬ ‫و‬ ‫ﻫﺎ‬‫آن‬ ‫ﻫﺎي‬‫ﻫﺎ‬
‫ﺑﺮاي‬ ‫ﮔﻮﻧﺎﮔﻮن‬‫ﺳﺒﮏ‬ ‫ﺣﺠﻢ‬ ‫ﻣﻘﺎﯾﺴﻪ‬‫داﻧﻪ‬‫ﺑ‬ ‫ﻫﺎ‬‫ﺎ‬
‫ـﺪ‬‫ـ‬‫ﺷ‬ ‫ـﻪ‬‫ـ‬‫ﺗﻬﯿ‬ ‫ـﺘﻦ‬‫ـ‬‫ﺑ‬ ‫ـﯽ‬‫ـ‬‫ﻓﯿﺰﯾﮑ‬ ‫ـﺎت‬‫ـ‬‫ﻣﺸﺨﺼ‬.‫ـﺮح‬‫ـ‬‫ﻃ‬ ‫ـﻦ‬‫ـ‬‫اﯾ‬ ‫در‬‫ـﺎ‬‫ـ‬‫ﻫ‬
‫ﻣﻘﺪار‬ ‫ﺑﻪ‬ ‫ﻫﺎ‬10‫ﻃﺒﯿﻌﯽ‬ ‫ﻣﺎﺳﻪ‬ ‫ﺑﺎ‬ ‫ﺣﺠﻤﺸﺎن‬ ‫درﺻﺪ‬
‫ﻣﺪرس‬ ‫ﻋﻤﺮان‬ ‫ﭘﮋوﻫﺸﯽ‬
81
‫ﺗﻮدﭼﯿﻨﯽ‬ ‫ﻣﻨﺤﻨﯽ‬]14[
‫اﺻﻼح‬ ‫ﻣﻨﺤﻨﯽ‬‫ﻫﻮﮔﻨﺴﺘﺎد‬ ‫ﺷﺪه‬]13[
‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺗﺤﻠﯿﻠﯽ‬ ‫ﺗﺨﻤﯿﻦ‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬
‫ﺗـﻨﺶ‬ ‫ﻣﻨﺤﻨـﯽ‬ ‫ﺗﺨﻤـﯿﻦ‬ ‫ﺑﺮاي‬ ‫رواﺑﻄﯽ‬-‫ﮐـﺮﻧﺶ‬
‫اﺳﺖ‬ ‫ﮐﺮده‬ ‫اراﺋﻪ‬ ‫ﭘﺎﯾﯿﻦ‬ ‫ﻫﺎي‬.‫ﺗﺨﻤﯿﻦ‬‫ﻫـﺎﯾﯽ‬
‫ﺳـﻦ‬ ‫و‬ ‫ﻣﻘﺎوﻣـﺖ‬ ،‫ﺳﯿﻤﺎن‬ ‫ﺑﻪ‬ ‫آب‬ ‫از‬ ‫ﺷﺪه‬
،‫ﻣﻮﺟـﻮد‬ ‫رواﺑـﻂ‬ ‫دﯾﮕـﺮ‬ ‫ﻃﺮﯾﻖ‬ ‫از‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﻪ‬ ‫ﻧﺴﺒﺖ‬ ‫اﺳﺖ‬ ‫زده‬
‫اﺳـﺖ‬ ‫ﮐـﺮده‬ ‫اراﺋﻪ‬ ‫ﺗﺮي‬.‫ﭼـﻮ‬ ‫و‬ ‫ﮐﺮﯾـﺮا‬]16[‫ﻧﯿـﺰ‬
‫اﻧﺪ‬.‫ﺑﻠﭽﻤﻦ‬]17[‫را‬ ‫ﻣﺘﻔـﺎوﺗﯽ‬ ‫رواﺑﻂ‬
‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﻧﺰوﻟﯽ‬ ‫و‬ ‫ﺻﻌﻮدي‬ ‫ﻫﺎي‬-‫اراﺋـﻪ‬ ‫ﮐﺮﻧﺶ‬
‫دارد‬ ‫ﻫﺪف‬ ‫دو‬ ‫ﭘﮋوﻫﺶ‬ ‫اﯾﻦ‬.‫از‬ ‫اﺳﺘﻔﺎده‬ ‫اﻣﮑﺎن‬ ‫اﺛﺒﺎت‬ ‫اﺑﺘﺪا‬
‫ﺳـﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﺗﻮﻟﯿﺪ‬ ‫در‬ ‫ﮐﺸﻮر‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫ﻟﯿﮑﺎي‬ ‫و‬ ‫اﺳﮑﻮرﯾﺎ‬‫داﻧـﻪ‬
‫ﻓـﻮق‬ ‫و‬ ‫ﻣﯿﮑﺮوﺳـﯿﻠﯿﺲ‬ ‫اﻓﺰودن‬ ‫ﺑﺎ‬ ‫ﭘﺮﻣﻘﺎوﻣﺖ‬‫روان‬‫در‬ ‫و‬ ‫ﮐﻨﻨـﺪه‬
‫ﮐﻮﺗﺎه‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫از‬ ‫ﺑﺮﺧﯽ‬ ‫ﺗﻌﯿﯿﻦ‬ ،‫ﺑﻌﺪ‬ ‫ﻣﺮﺣﻠﻪ‬
‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﮐﺸﺸﯽ‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻣﺎﻧﻨﺪ‬ ‫ﺑﺘﻦ‬ ‫اﯾﻦ‬
‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺑﺮرﺳﯽ‬ ‫و‬
2-‫آزﻣﺎﯾﺸﮕﺎﻫﯽ‬ ‫اﻃﻼﻋﺎت‬
1-2-‫ﻣﺼﺮﻓﯽ‬ ‫ﻣﺼﺎﻟﺢ‬
‫ـﻪ‬‫ـ‬‫ﻧﻤﻮﻧ‬ ‫ـﮥ‬‫ـ‬‫ﻫﻤ‬ ‫ﺳـﺎﺧﺖ‬ ‫در‬
،‫ازﻧـﺎ‬ ‫در‬ ‫واﻗـﻊ‬ ‫اﯾـﺮان‬ ‫ﻓﺮوآﻟﯿـﺎژ‬ ‫ﺻـﻨﺎﯾﻊ‬ ‫ﺷﺮﮐﺖ‬ ‫در‬ ‫ﺗﻮﻟﯿﺪﺷﺪه‬
‫درﺷﺖ‬ ‫ﻟﯿﮑﺎي‬‫اﺳﺘﺨﺮاج‬ ‫اﺳﮑﻮرﯾﺎي‬ ‫و‬ ‫اﯾﺮاﻧﯽ‬ ‫داﻧﻪ‬
‫اﻧﺪازه‬ ‫ﺑﯿﺸﯿﻨﮥ‬ ‫ﺑﺎ‬5/12
‫ـﯽ‬‫ـ‬‫اﻓﺰودﻧ‬ ‫ـﯿﻦ‬‫ـ‬‫ﻫﻤﭽﻨ‬ ‫و‬ ‫ـﺎك‬‫ـ‬‫ﻣﺘﻮﺳ‬ ‫ـﺮﮐﺖ‬‫ـ‬‫ﺷ‬ ‫ـﺪي‬‫ـ‬‫ﺗﻮﻟﯿ‬ ‫ـﻮﻟﯽ‬‫ـ‬‫ﻣﻌﻤ‬
‫ﻓﻮق‬‫روان‬‫ﻣﺤ‬ ،‫ﻧﻔﺘﺎﻟﯿﻦ‬ ‫ﭘﺎﯾﻪ‬ ‫ﺑﺮ‬ ‫ﮐﻨﻨﺪه‬
‫ﺷﺪ‬ ‫اﺳﺘﻔﺎده‬ ‫اﯾﺮاﻧﯿﺎن‬ ‫اف‬
‫درﺷﺖ‬ ‫و‬ ‫ﻣﻌﻤﻮﻟﯽ‬‫اﺳـﺖ‬ ‫ﺷـﺪه‬ ‫اﺳـﺘﻔﺎده‬ ‫ﺧﺸـﮏ‬ ‫ﺳـﺒﮏ‬ ‫داﻧﻪ‬
‫داﻧﻪ‬‫وزﻧـﯽ‬ ‫ﺑﻨﺪي‬)‫ردﺷـﺪه‬ ‫درﺻـﺪ‬
‫ـﺘﺎﻧﺪارد‬‫ـ‬‫اﺳ‬ ‫ـﺪوده‬‫ـ‬‫ﻣﺤ‬ ‫در‬ ‫ـﮑﻮرﯾﺎ‬‫ـ‬‫اﺳ‬
‫داﺷﺖ‬.‫ﻓﻮق‬ ‫و‬ ‫ﺳﯿﻤﺎن‬
‫ـﺮ‬‫ـ‬‫ﺑ‬ ‫ـﻖ‬‫ـ‬‫ﻣﻨﻄﺒ‬ASTM C150
‫اﺳﺖ‬.‫اﻧﺒﻮﻫﯽ‬ ‫ﺧﺸﮏ‬ ‫ﻓﻀﺎﯾﯽ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬
‫ﺗﺮﺗﯿـﺐ‬ ‫ﺑـﻪ‬ ‫اﺳـﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬
‫ﻣﯿﻠـﻪ‬ ‫ﺑﺎ‬ ‫ﻣﺘﺮاﮐﻢ‬ ‫ﺧﺸﮏ‬ ‫ﻓﻀﺎﯾﯽ‬
‫اﺳﺖ‬.‫اﻧﺒﻮﻫﯽ‬ ‫ﺧﺸﮏ‬ ‫ﻓﻀﺎﯾﯽ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﻣﯿﺰان‬ ‫ﺑﯿﺸﺘﺮﯾﻦ‬
‫درﺷﺖ‬ ‫ﺑﺮاي‬‫داﻧﻪ‬‫اﺳـﺘﺎﻧﺪارد‬ ‫ﻃﺒـﻖ‬ ‫ﺳـﺒﮏ‬ ‫ﻫﺎي‬
(3Kg/m)880‫اﺳﺖ‬ ‫ﺷﺪه‬ ‫ﻗﯿﺪ‬
‫ﺗﺮﺗﯿﺐ‬ ‫ﺑﻪ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬
2-2-‫ﻣﺨﻠﻮط‬ ‫اﻧﺘﺨﺎب‬ ‫اﺻﻮل‬
‫ﻣﺨﻠﻮط‬ ‫ﺷﺶ‬‫ﺑﺮاي‬ ‫ﮔﻮﻧﺎﮔﻮن‬
‫ـﺪ‬‫ـ‬‫ﺷ‬ ‫ـﻪ‬‫ـ‬‫ﺗﻬﯿ‬ ‫ـﺘﻦ‬‫ـ‬‫ﺑ‬ ‫ـﯽ‬‫ـ‬‫ﻓﯿﺰﯾﮑ‬ ‫ـﺎت‬‫ـ‬‫ﻣﺸﺨﺼ‬
‫ﺳﺒﮏ‬‫داﻧﻪ‬‫ﻣﻘﺪار‬ ‫ﺑﻪ‬ ‫ﻫﺎ‬
‫ﻋﻠﻤﯽ‬ ‫ﻣﺠﻠﻪ‬-‫ﻣﺪرس‬ ‫ﻋﻤﺮان‬ ‫ﭘﮋوﻫﺸﯽ‬
‫ﺗﻮدﭼﯿﻨﯽ‬ ‫ﻣﻨﺤﻨﯽ‬
‫اﺻﻼح‬ ‫ﻣﻨﺤﻨﯽ‬
‫ﺷﮑﻞ‬)1(‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺗﺤﻠﯿﻠﯽ‬ ‫ﺗﺨﻤﯿﻦ‬
‫ﭘﻮﭘﻮوﯾﭻ‬]15[‫ﺗـﻨﺶ‬ ‫ﻣﻨﺤﻨـﯽ‬ ‫ﺗﺨﻤـﯿﻦ‬ ‫ﺑﺮاي‬ ‫رواﺑﻄﯽ‬
‫ﺑﺘﻦ‬‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﺎ‬ ‫ﻫﺎي‬‫اﺳﺖ‬ ‫ﮐﺮده‬ ‫اراﺋﻪ‬ ‫ﭘﺎﯾﯿﻦ‬ ‫ﻫﺎي‬
‫داده‬ ‫داﻣﻨﻪ‬ ‫در‬ ‫وي‬ ‫ﮐﻪ‬‫ﺳـﻦ‬ ‫و‬ ‫ﻣﻘﺎوﻣـﺖ‬ ،‫ﺳﯿﻤﺎن‬ ‫ﺑﻪ‬ ‫آب‬ ‫از‬ ‫ﺷﺪه‬
،‫ﻣﻮﺟـﻮد‬ ‫رواﺑـﻂ‬ ‫دﯾﮕـﺮ‬ ‫ﻃﺮﯾﻖ‬ ‫از‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﻪ‬ ‫ﻧﺴﺒﺖ‬ ‫اﺳﺖ‬ ‫زده‬
‫ﻣﻨﻄﻘﯽ‬ ‫ﻧﺘﺎﯾﺞ‬‫اﺳـﺖ‬ ‫ﮐـﺮده‬ ‫اراﺋﻪ‬ ‫ﺗﺮي‬
‫ارا‬ ‫دﯾﮕﺮي‬ ‫راﺑﻄﻪ‬‫ﮐﺮده‬ ‫ﺋﻪ‬‫اﻧﺪ‬
‫ﺷﺎﺧﻪ‬ ‫ﺑﺮاي‬‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﻧﺰوﻟﯽ‬ ‫و‬ ‫ﺻﻌﻮدي‬ ‫ﻫﺎي‬
‫اﺳﺖ‬ ‫ﮐﺮده‬.
‫دارد‬ ‫ﻫﺪف‬ ‫دو‬ ‫ﭘﮋوﻫﺶ‬ ‫اﯾﻦ‬
‫ﺳـﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﺗﻮﻟﯿﺪ‬ ‫در‬ ‫ﮐﺸﻮر‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫ﻟﯿﮑﺎي‬ ‫و‬ ‫اﺳﮑﻮرﯾﺎ‬
‫ﻓـﻮق‬ ‫و‬ ‫ﻣﯿﮑﺮوﺳـﯿﻠﯿﺲ‬ ‫اﻓﺰودن‬ ‫ﺑﺎ‬ ‫ﭘﺮﻣﻘﺎوﻣﺖ‬
‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫و‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﺮرﺳﯽ‬-‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫داﻧﻪ‬‫ﭼﺎﻟﻪ‬ ‫ﻋﻠﯿﺮﺿﺎ‬ ‫و‬ ‫ﺧﺎﻧﺰادي‬ ‫ﻣﺼﻄﻔﯽ‬‫ﮐﺎﯾﯽ‬
82
‫ﺷﺪ‬ ‫ﺟﺎﯾﮕﺰﯾﻦ‬.‫ﺣﺮوف‬L‫و‬S‫اﺧـﺘﻼط‬ ‫ﻃـﺮح‬ ‫ﻫﺮ‬ ‫ﻋﻨﻮان‬ ‫در‬
‫اﺳـﺖ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﺑﺘﻦ‬ ‫ﺑﯿﺎﻧﮕﺮ‬ ‫ﺗﺮﺗﯿﺐ‬ ‫ﺑﻪ‬.‫ﻫﻤـﮥ‬
‫ﻣﺨﻠﻮط‬‫ﺑﺎ‬ ‫ﺑﺘﻦ‬ ‫ﻫﺎي‬500‫ﺑـﺮ‬ ‫ﮐﯿﻠـﻮﮔﺮم‬‫ﻣـﻮاد‬ ‫ﻣﮑﻌـﺐ‬ ‫ﻣﺘـﺮ‬
‫ﺳﯿﻤﺎﻧﯽ‬ ‫ﻣﻮاد‬ ‫ﺑﻪ‬ ‫ﺳﯿﻤﺎن‬ ‫وزﻧﯽ‬ ‫ﻧﺴﺒﺖ‬ ‫و‬ ‫ﺳﯿﻤﺎﻧﯽ‬3/0‫ﻃـﺮح‬
‫ﺷﺪ‬.‫ﻃﺮح‬ ‫اﯾﻦ‬ ‫در‬‫ﻫﺎ‬450‫ﻧﻮع‬ ‫ﭘﺮﺗﻠﻨﺪ‬ ‫ﺳﯿﻤﺎن‬ ‫ﮐﯿﻠﻮﮔﺮم‬I‫ﺑﺎ‬
50‫ﺷﺪ‬ ‫اﺳﺘﻔﺎده‬ ‫ﺳﯿﻠﯿﺴﯽ‬ ‫دوده‬ ‫ﮐﯿﻠﻮﮔﺮم‬.‫ﻣﺨﻠﻮط‬ ‫ﻫﻤﮥ‬ ‫از‬‫ﻫﺎ‬
‫اﺳـﻼﻣﭗ‬ ‫اﻓﺖ‬ ‫ﻣﯿﺰان‬ ‫ﮐﻪ‬ ‫ﺷﺪ‬ ‫ﮔﺮﻓﺘﻪ‬ ‫اﺳﻼﻣﭗ‬ ‫اﻓﺖ‬ ‫آزﻣﺎﯾﺶ‬
‫اﺧﺘﻼط‬ ‫ﻫﻤﮥ‬ ‫در‬‫ﻫﺎ‬10-8‫ﺳـﺎﻧﺘﯽ‬‫اﺳـﺖ‬ ‫ﺑـﻮده‬ ‫ﻣﺘـﺮ‬.‫ﺑـﺮ‬‫اي‬
‫ﻓﻮق‬ ،‫ﻣﻮردﻧﻈﺮ‬ ‫ﮐﺎراﯾﯽ‬ ‫ﺑﻪ‬ ‫دﺳﺘﯿﺎﺑﯽ‬‫روان‬‫ﮐﻨﻨﺪه‬‫ﻣﯿـﺰان‬ ‫ﺑـﻪ‬ ‫اي‬
‫ﺑـﺘﻦ‬ ‫ﺑـﻪ‬ ‫ﺳـﯿﻤﺎن‬ ‫وزن‬ ‫درﺻﺪ‬ ‫ﯾﮏ‬‫ﺷـﺪ‬ ‫اﺿـﺎﻓﻪ‬ ‫ﻫـﺎ‬.‫ﻫـﺮ‬ ‫از‬
‫ﻧﻤﻮﻧـﻪ‬ ،‫اﺧﺘﻼط‬‫ﻣﮑﻌـﺐ‬ ‫ﻫـﺎي‬150‫ﻣﯿﻠـﯽ‬‫ﺳـﯿﻠﻨﺪر‬ ،‫ﻣﺘـﺮي‬
‫ﻃـﻮل‬ ‫ﺑﺎ‬ ‫ﺳﯿﻠﻨﺪر‬ ‫و‬ ‫اﺳﺘﺎﻧﺪارد‬200‫ﻗﻄـﺮ‬ ‫و‬100‫ﻣﯿﻠـﯽ‬‫ﻣﺘـﺮ‬
‫ﺳـﻦ‬ ‫در‬ ‫اﻻﺳﺘﯿﺴـﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺗﻌﯿﯿﻦ‬ ‫ﺑﺮاي‬
28‫ﺷ‬ ‫ﺗﻬﯿﻪ‬ ‫روز‬‫ﺪ‬.‫ﻧﻤﻮﻧـﻪ‬ ‫ﻫﻤـﮥ‬‫ﻣﯿـﺰ‬ ‫روي‬ ‫ﻻﯾـﻪ‬ ‫دو‬ ‫در‬ ‫ﻫـﺎ‬
‫ﺷﺪ‬ ‫ﻣﺘﺮاﮐﻢ‬ ‫وﯾﺒﺮه‬.‫آن‬ ‫ﺳﻄﺢ‬‫ﺗـﺮاز‬ ‫ﺷـﺪن‬ ‫ﻣﺘﺮاﮐﻢ‬ ‫از‬ ‫ﭘﺲ‬ ‫ﻫﺎ‬
‫ﻗﺎﻟـﺐ‬ ‫در‬ ‫روز‬ ‫ﯾـﮏ‬ ‫ﻣﺪت‬ ‫ﺑﻪ‬ ‫و‬ ‫ﺷﺪ‬ ‫ﭘﺮداﺧﺖ‬ ‫ﻣﺎﻟﻪ‬ ‫ﺑﺎ‬ ،‫ﺷﺪه‬
‫ﻧﮕﻪ‬‫ﻗﺎﻟﺐ‬ ‫ﺳﭙﺲ‬ ‫ﺷﺪ؛‬ ‫داري‬‫ﻧﻤﻮﻧﻪ‬ ‫و‬ ‫ﺷﺪ‬ ‫ﺑﺎز‬ ‫ﻫﺎ‬‫زﻣـﺎن‬ ‫ﺗـﺎ‬ ‫ﻫﺎ‬
‫دﻣـﺎي‬ ‫ﺑـﺎ‬ ‫آب‬ ‫ﺣﻮﺿـﭽﻪ‬ ‫در‬ ‫آزﻣـﺎﯾﺶ‬ ‫اﻧﺠﺎم‬2±23‫درﺟـﻪ‬
‫ﺳﺎﻧﺘﯽ‬‫ﻋﻤﻞ‬ ‫ﮔﺮاد‬‫ﺷﺪ‬ ‫آوري‬.
‫ﺟﺪول‬)1(‫ﻧﺴﺒﺖ‬ ‫و‬ ‫ﻣﻘﺎدﯾﺮ‬‫ﻣﺨﻠﻮط‬ ‫اﺟﺰاء‬ ‫ﻫﺎي‬‫آزﻣﺎﯾﺶ‬ ‫ﻫﺎي‬(3Kg/m)
‫ﻧﺎم‬
‫اﺧﺘﻼط‬
‫ﺳﯿﻤﺎن‬‫ﻣﯿﮑﺮوﺳﯿﻠﯿﺲ‬‫درﺷﺖ‬‫داﻧﻪ‬‫رﯾﺰداﻧﻪ‬
‫آب‬
‫آزاد‬
‫وزن‬
‫ﻣﺨﺼﻮص‬
‫ﺗﺎزه‬ ‫ﺑﺘﻦ‬
L1450503157301501715
L2450502608601501790
L3450502059901501865
S1450505957281501998
S2450505018581502034
S3450504079881502070
‫ﻧﺴﺒﺖ‬‫ﭘﯿﺸﻨﻬﺎدﺷـﺪه‬ ‫ﺷـﯿﻮه‬ ‫اﺳـﺎس‬ ‫ﺑﺮ‬ ‫اﺑﺘﺪا‬ ‫در‬ ‫ﺑﺘﻦ‬ ‫اﺧﺘﻼط‬ ‫ﻫﺎي‬
‫در‬ACI 211.1]21[‫ﺷﺪ‬ ‫ﻣﻨﻈﻮر‬.‫ﺑﻪ‬ ‫رﺳﯿﺪن‬ ‫ﺗﺎ‬ ‫ﻣﻘﺎدﯾﺮ‬ ‫اﯾﻦ‬ ‫ﺳﭙﺲ‬
‫ـﺪ‬‫ـ‬‫ﺷ‬ ‫ـﻪ‬‫ـ‬‫ﺑﻬﯿﻨ‬ ‫ـﺮ‬‫ـ‬‫ﻧﻈ‬ ‫ـﻮرد‬‫ـ‬‫ﻣ‬ ‫ـﺎري‬‫ـ‬‫ﻓﺸ‬ ‫ـﺖ‬‫ـ‬‫ﻣﻘﺎوﻣ‬.‫ـﺒﺖ‬‫ـ‬‫ﻧﺴ‬ ‫و‬ ‫ـﺎدﯾﺮ‬‫ـ‬‫ﻣﻘ‬
‫ﻣﺨﻠﻮط‬‫ﺟﺪول‬ ‫در‬ ‫ﺑﺘﻦ‬ ‫ﻫﺎي‬)1(‫ﻣﯽ‬ ‫دﯾﺪه‬‫ﺷﻮد‬.
3-‫آن‬ ‫ﺗﻔﺴﯿﺮ‬ ‫و‬ ‫ﻧﺘﺎﯾﺞ‬‫ﻫﺎ‬
3-1-‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬
‫ﻧﻤﻮﻧﻪ‬‫اﺳﺘﺎﻧﺪارد‬ ‫اﺳﺘﻮاﻧﻪ‬ ‫ﻫﺎي‬150×300‫ﻣﯿﻠـﯽ‬‫ﻣﮑﻌـﺐ‬ ‫و‬ ‫ﻣﺘـﺮ‬
150‫ﻣﯿﻠﯽ‬‫ﺳـﻦ‬ ‫در‬ ‫ﻓﺸـﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫آزﻣﺎﯾﺶ‬ ‫و‬ ‫ﺳﺎﺧﺘﻪ‬ ‫ﻣﺘﺮي‬
28‫ﺷـﺪ‬ ‫اﻧﺠﺎم‬ ‫آن‬ ‫روي‬ ‫روز‬.‫آزﻣـﺎﯾﺶ‬ ‫ﻧﺘـﺎﯾﺞ‬‫ﻣﻘﺎوﻣـﺖ‬ ‫ﻫـﺎي‬
‫ﻧﻤﻮﻧﻪ‬ ‫روي‬ ‫ﻓﺸﺎري‬‫ﻫﺎي‬28‫ﻣﮑﻌﺐ‬ ‫روزه‬15‫ﺳـﺎﻧﺘﯽ‬‫و‬ ‫ﻣﺘـﺮي‬
‫ﻧﻤﻮ‬ ‫ﺧﺸﮏ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﻧﯿﺰ‬ ‫و‬ ‫اﺳﺘﺎﻧﺪارد‬ ‫اﺳﺘﻮاﻧﻪ‬‫ﻧـﻪ‬‫در‬ ‫ﻫـﺎ‬
‫ﺟﺪول‬)2(‫اﺳﺖ‬ ‫ﺷﺪه‬ ‫اراﺋﻪ‬.
‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﯿﺸﺘﺮﯾﻦ‬28‫ﺑـﺘﻦ‬ ‫روزه‬‫ﺣـﺎوي‬ ‫ﻫـﺎي‬
‫ﻃﺮح‬ ،‫ﻟﯿﮑﺎ‬L3‫اﺳﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫در‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬‫اي‬MPa4/38‫و‬
‫ﻣﮑﻌﺒﯽ‬ ‫ﻧﻤﻮﻧﻪ‬MPa85/40‫ﺑﻪ‬‫اﺳـﺖ‬ ‫آﻣـﺪه‬ ‫دﺳﺖ‬.‫اﯾـﻦ‬ ‫در‬
‫ﺧﺸﮏ‬ ‫ﺑﺘﻦ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﺣﺎﻟﺖ‬kg/m31735‫ﺑـﻪ‬‫دﺳـﺖ‬
‫ـﺖ‬‫ـ‬‫اﺳ‬ ‫ـﺪه‬‫ـ‬‫آﻣ‬.‫ـﺎري‬‫ـ‬‫ﻓﺸ‬ ‫ـﺖ‬‫ـ‬‫ﻣﻘﺎوﻣ‬ ‫ـﺘﺮﯾﻦ‬‫ـ‬‫ﺑﯿﺸ‬28‫ـﯿﻦ‬‫ـ‬‫ﺑ‬ ‫روزه‬
‫ﺑ‬‫ﺘﻦ‬‫ﻣﺨﻠﻮط‬ ‫ﺑﻪ‬ ‫ﻣﺮﺑﻮط‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬S3‫ﮐـﻪ‬ ‫اﺳـﺖ‬
‫ـﺮ‬‫ـ‬‫ﺑﺮاﺑ‬ ‫ـﯽ‬‫ـ‬‫ﻣﮑﻌﺒ‬ ‫ـﻪ‬‫ـ‬‫ﻧﻤﻮﻧ‬ ‫ـﺮاي‬‫ـ‬‫ﺑ‬MPa63/54‫ـﻪ‬‫ـ‬‫ﻧﻤﻮﻧ‬ ‫ـﺮاي‬‫ـ‬‫ﺑ‬ ‫و‬
‫اﺳﺘﻮاﻧﻪ‬‫ﺑﺮاﺑﺮ‬ ‫اي‬MPa62/48‫اﺳـﺖ‬.‫ﺑـﺘﻦ‬ ‫ﻣﺨﺼـﻮص‬ ‫وزن‬
‫ﺧﺸﮏ‬‫ﺣـﺪود‬ ‫ﻃـﺮح‬ ‫اﯾـﻦ‬ ‫ﺑـﻪ‬ ‫ﻣﺮﺑـﻮط‬ ‫ﺷـﺪه‬kg/m31940
‫ﺑﻪ‬‫اﺳﺖ‬ ‫آﻣﺪه‬ ‫دﺳﺖ‬.‫ﻣﻘﺎوﻣﺖ‬ ‫ﻧﺘﺎﯾﺞ‬‫ﻓﺸـﺎري‬ ‫ﻫﺎي‬28‫روزه‬
‫آزﻣﻮﻧﻪ‬ ‫وزن‬ ‫ﺗﺎﺑﻊ‬ ً‫ﻼ‬‫ﻋﻤ‬‫ﺑ‬ ‫و‬ ‫اﺳﺖ‬ ‫ﻫﺎ‬‫ﻣﻘﺎوﻣـﺖ‬ ،‫آن‬ ‫ﮐـﺎﻫﺶ‬ ‫ﺎ‬
‫ﻣﯽ‬ ‫ﮐﺎﻫﺶ‬ ‫ﻧﯿﺰ‬‫ﯾﺎﺑﺪ‬.‫ﻧﻤﻮﻧـﻪ‬ ‫ﻓﺸـﺎري‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﻧﺴﺒﺖ‬‫ﻫـﺎي‬
‫اﺳﺘﻮاﻧﻪ‬‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬ ‫ﻣﮑﻌﺐ‬ ‫ﺑﻪ‬ ‫اي‬‫ﺣـﺪود‬ ‫ﻟﯿﮑـﺎ‬ ‫ﺣـﺎوي‬ ‫ﻫـﺎي‬
93/0‫ﻧﻤﻮﻧﻪ‬ ‫ﺑﺮاي‬ ‫و‬‫ﺣﺪود‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬87/0‫ﺛﺒﺖ‬
‫اﺳـﺖ‬ ‫ﺷﺪه‬.‫ﻧﮑـﺎت‬ ‫رﻋﺎﯾـﺖ‬ ‫ﺑـﺎ‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﺑﯿﺸـﺘﺮ‬ ‫اﻓـﺰاﯾﺶ‬
‫ﻣﺤﺪوده‬ ‫در‬ ‫ﺧﺸﮏ‬ ‫ﺑﺘﻦ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﺣﻔﻆ‬ ‫و‬ ‫اﻗﺘﺼﺎدي‬
‫ﺑﺘﻦ‬‫ﺳـﺒﮏ‬ ‫ﻫﺎي‬‫ﻧﯿﺴـﺖ‬ ‫ﻣﻘـﺪور‬ ً‫ﻼ‬‫ﻋﻤـ‬.‫ﻣﻘﺎوﻣـﺖ‬ ‫اﻓـﺰاﯾﺶ‬
‫ﺑﺘﻦ‬‫ﺗﺤﻘﯿﻘـﺎت‬ ‫ﺑـﻪ‬ ‫ﻧﺴﺒﺖ‬ ‫ﭘﮋوﻫﺶ‬ ‫اﯾﻦ‬ ‫در‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬
‫داﻧﻪ‬ ‫ﻧﻮع‬ ‫ﺗﻔﺎوت‬ ‫دﻟﯿﻞ‬ ‫ﺑﻪ‬ ‫اﯾﺮان‬ ‫در‬ ‫ﮔﺬﺷﺘﻪ‬‫ﻟﯿﮑﺎﻫـﺎي‬ ‫ﺑـﺎ‬ ‫ﻫـﺎ‬
‫اﺳﺘﻔﺎده‬‫اﺳﺖ‬ ‫ﺗﺤﻘﯿﻘﺎت‬ ‫آن‬ ‫در‬ ‫ﺷﺪه‬.
‫ﻋﻠﻤﯽ‬ ‫ﻣﺠﻠﻪ‬-‫ﻣﺪرس‬ ‫ﻋﻤﺮان‬ ‫ﭘﮋوﻫﺸﯽ‬‫ﺷﻤﺎره‬ ،‫دوازدﻫﻢ‬ ‫دوره‬4/‫زﻣﺴﺘﺎن‬1391
83
‫ﺟﺪول‬)2(‫آزﻣﺎﯾﺶ‬ ‫ﻧﺘﺎﯾﺞ‬‫ﻧﻤﻮﻧﻪ‬ ‫روي‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻫﺎي‬‫ﻣﮑﻌﺐ‬ ‫ﻫﺎي‬
15‫ﺳﺎﻧﺘﯽ‬‫اﺳﺘﺎﻧﺪارد‬ ‫اﺳﺘﻮاﻧﻪ‬ ‫و‬ ‫ﻣﺘﺮي‬
‫ﻧﺎم‬
‫ﻃﺮح‬
‫ﻣﻘﺎوﻣﺖ‬
‫ﻣﮑﻌﺐ‬ ‫ﻓﺸﺎري‬
(MPa)
‫ﻣﻘﺎوﻣﺖ‬
‫ﻓﺸﺎري‬
‫اﺳﺘﻮاﻧﻪ‬(MPa)
‫وزن‬
‫ﻣﺨﺼﻮص‬
‫ﺧﺸﮏ‬
(3Kg/m)
‫ﻣﻘﺎوﻣﺖ‬ ‫ﻧﺴﺒﺖ‬
‫ﻧﻤﻮﻧﻪ‬‫اﺳﺘﻮاﻧﻪ‬ ‫ﻫﺎي‬
‫ﻣﮑﻌﺐ‬ ‫ﺑﻪ‬
L120/3354/30158592/0
L229/3675/33166093/0
L385/4040/38173594/0
S135/4500/39186886/0
S246/5090/43190487/0
S363/5462/48194089/0
‫داﻧﻪ‬ ،‫ﻟﯿﮑﺎ‬ ‫ﺷﺮﮐﺖ‬ ‫ﺗﻮﻟﯿﺪﮐﻨﻨﺪﮔﺎن‬ ‫اﻇﻬﺎر‬ ‫ﺑﻪ‬ ‫ﺑﻨﺎ‬‫ﺷﺪه‬ ‫اﺳﺘﻔﺎده‬ ‫ﻫﺎي‬
‫دارﻧﺪ‬ ‫ﺑﻬﺘﺮي‬ ‫ﮐﯿﻔﯿﺖ‬ ‫ﭘﮋوﻫﺶ‬ ‫اﯾﻦ‬ ‫در‬.
‫ﺳﺒﮏ‬ ‫اﺷﻐﺎل‬ ‫ﺣﺠﻢ‬ ‫ﺗﺄﺛﯿﺮ‬‫داﻧﻪ‬‫ﺧـﻮﺑﯽ‬ ‫ﺑـﻪ‬ ‫ﻧﯿـﺰ‬ ‫ﺑﺘﻦ‬ ‫در‬ ‫ﻫﺎ‬
‫ﻣﯽ‬ ‫دﯾﺪه‬‫ﺷﻮد‬.‫درﺷﺖ‬ ‫ﺑﺎﻓﺖ‬‫ﺳـﺒﮏ‬ ‫اﻓـﺰاﯾﺶ‬ ‫ﯾﻌﻨـﯽ‬ ‫ﺗﺮ‬‫داﻧـﻪ‬
‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫داﺷﺘﻪ‬ ‫ﻧﺘﯿﺠﻪ‬ ‫دو‬ ،‫ﻣﻌﻤﻮﻟﯽ‬ ‫ﻣﺎﺳﻪ‬ ‫ﮐﺎﻫﺶ‬ ‫و‬ ‫درﺷﺖ‬
‫ﻓﺸـﺎري‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﮐـﺎﻫﺶ‬ ‫و‬ ‫ﺑـﺘﻦ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﮐﺎﻫﺶ‬
‫ﺳـﻨﮓ‬ ‫ﺑﺨـﺶ‬ ‫در‬ ‫ﺗﺨﻠﺨﻞ‬ ‫و‬ ‫ﭘﻮﮐﯽ‬ ‫زﯾﺮا‬ ‫اﺳﺖ؛‬‫ﺑﯿﺸـﺘﺮ‬ ‫داﻧـﻪ‬
‫اﺳـﺖ‬ ‫ﺷﺪه‬ ‫اﯾﺠﺎد‬ ‫ﺑﯿﺸﺘﺮي‬ ‫ﺿﻌﻒ‬ ‫و‬ ‫ﺷﺪه‬.‫ﻣﻘـﺪار‬ ‫ﮐـﺎﻫﺶ‬
‫ﺳﺒﮏ‬‫ﻣﺨﻠـﻮط‬ ‫ﻃـﺮح‬ ‫روش‬ ‫از‬ ‫اﺳـﺘﻔﺎده‬ ‫ﺑـﻪ‬ ‫ﺗﻮﺟـﻪ‬ ‫ﺑـﺎ‬ ‫داﻧﻪ‬
‫درﺷـﺖ‬ ‫ﻣﻘﺪار‬ ‫ﺗﻌﯿﯿﻦ‬ ‫ﺑﺨﺶ‬ ‫در‬ ‫آﻣﺮﯾﮑﺎﯾﯽ‬‫اﻓـﺰاﯾﺶ‬ ‫و‬ ‫داﻧـﻪ‬
‫ـﺒﮏ‬‫ـ‬‫ﺳ‬ ‫ـﻦ‬‫ـ‬‫ﺷ‬ ‫ـﺎﻫﺶ‬‫ـ‬‫ﮐ‬ ‫ـﻞ‬‫ـ‬‫دﻟﯿ‬ ‫ـﻪ‬‫ـ‬‫ﺑ‬ ‫ـﻮﻟﯽ‬‫ـ‬‫ﻣﻌﻤ‬ ‫ـﻪ‬‫ـ‬‫ﻣﺎﺳ‬ ‫ـﺪار‬‫ـ‬‫ﻣﻘ‬‫و‬
‫ﺑﻪ‬‫ﭼﺸـﻢ‬ ‫اﻓـﺰاﯾﺶ‬ ‫ﺳﺒﺐ‬ ‫ﻣﻄﻠﻖ‬ ‫ﺣﺠﻢ‬ ‫ﻓﺮﻣﻮل‬ ‫ﮐﺎرﮔﯿﺮي‬‫ﮔﯿـﺮ‬
‫ﻣﯽ‬ ‫ﺑﺘﻦ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬‫ﺑـﺎﻻﺗﺮ‬ ‫ﻓﺸـﺎري‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫و‬ ‫ﺷـﻮد‬
‫ﻣﯽ‬‫رود‬.‫ﻣﯽ‬ ‫را‬ ‫دﯾﮕﺮ‬ ‫دﻟﯿﻞ‬ ‫اﻣﺎ‬‫ﮐﯿﻔﯿـﺖ‬ ‫رﻓـﺘﻦ‬ ‫ﺑـﺎﻻ‬ ‫در‬ ‫ﺗـﻮان‬
‫ﺳﺒﮏ‬‫داﻧﺴﺖ‬ ‫درﺷﺖ‬ ‫داﻧﻪ‬.‫آزﻣﺎﯾﺶ‬ ‫ﻧﺘﺎﯾﺞ‬ ‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬ ‫ﺑﺎ‬‫ﻫـﺎي‬
‫ﻣﯽ‬ ‫ﻧﻈﺮ‬ ‫ﺑﻪ‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬‫ﺳﯿﻠﯿﺴـﯽ‬ ‫دوده‬ ‫ﻣﺼـﺮف‬ ‫رﺳـﺪ‬
‫ﺑـﺘﻦ‬ ‫ﺑـﺮ‬ ‫ﺧـﻮﺑﯽ‬ ‫ﺗﺄﺛﯿﺮ‬‫ﻫـﺎ‬‫آزﻣـﺎﯾﺶ‬ ‫ي‬‫اﺳـﺖ‬ ‫داﺷـﺘﻪ‬ ‫ﺷـﺪه‬.
‫ﺗﺤﻠﯿﻞ‬‫ﻣﻨﻄﻘـﻪ‬ ‫ﺑﻬﺒـﻮد‬ ‫در‬ ‫ﺑﺎﯾـﺪ‬ ‫را‬ ‫ﻋﻠﺖ‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫ﻣﺪﻋﯽ‬ ‫ﮔﺮ‬
‫ﺑﻪ‬ ‫ﺗﻤﺎس‬‫ﺟﺴـﺖ‬ ‫ﺳﯿﻠﯿﺴـﯽ‬ ‫دوده‬ ‫وﺳـﯿﻠﮥ‬‫ﮐـﺮد‬ ‫وﺟـﻮ‬.‫دوده‬
‫ﻣـﯽ‬ ‫اﺟـﺎزه‬ ‫ﺳﯿﻠﯿﺴﯽ‬‫ﻧﺰدﯾﮑـﯽ‬ ‫در‬ ‫ﺑﺘﻮاﻧـﺪ‬ ‫ﻣـﺎده‬ ‫اﯾـﻦ‬ ‫دﻫـﺪ‬
‫ﺳﺒﮏ‬‫ﻫﯿﺪروﮐﺴـﯿﺪ‬ ‫ﺑﻠﻮرﻫـﺎي‬ ‫از‬ ‫ﺗـﻮﺟﻬﯽ‬ ‫ﻗﺎﺑﻞ‬ ‫ﻣﻘﺎدﯾﺮ‬ ‫داﻧﻪ‬
‫ﻣﺤﺼـﻮﻻت‬ ‫و‬ ‫رﺳـﺎﻧﺪ‬ ‫ﻣﺼﺮف‬ ‫ﺑﻪ‬ ‫و‬ ‫ﮐﺮده‬ ‫ﺟﺬب‬ ‫را‬ ‫ﮐﻠﺴﯿﻢ‬
‫ﻧﻔ‬‫ﻣﻘﺎوم‬ ‫و‬ ‫ﻮذﻧﺎﭘﺬﯾﺮﺗﺮ‬‫ﺷﻮد‬ ‫ﺣﺎﺻﻞ‬ ‫ﺗﺮي‬.‫در‬ ‫رﻃﻮﺑﺖ‬ ‫وﺟﻮد‬
‫ﺳﺒﮏ‬‫ﻋﻤـﻞ‬ ‫ﻣﺴﺌﻠﻪ‬ ‫و‬ ‫داﻧﻪ‬‫ﮐﻤـﮏ‬ ‫ﻧﯿـﺰ‬ ‫داﺧﻠـﯽ‬ ‫آوري‬‫ﮐﻨﻨـﺪه‬
‫اﺳﺖ‬.‫ﺑﻪ‬ ‫ﻧﺘﺎﯾﺞ‬ ‫در‬ ‫ﺗﻮﺟﻪ‬ ‫ﻗﺎﺑﻞ‬ ‫ﻧﮑﺘﻪ‬‫دﺳﺖ‬‫ﻣﻘﺎوﻣـﺖ‬ ‫از‬ ‫آﻣﺪه‬
‫ﻧﻤﻮﻧﻪ‬ ‫ﻓﺸﺎري‬‫اﺳﺘﻮاﻧﻪ‬ ‫و‬ ‫ﻣﮑﻌﺒﯽ‬ ‫ﻫﺎي‬‫ﻣﻘﺎوﻣـﺖ‬ ‫ﻧﺴـﺒﺖ‬ ،‫اي‬
‫اﺳﺘﻮاﻧﻪ‬‫اﺳـﺖ‬ ‫ﻣﮑﻌﺒـﯽ‬ ‫ﺑﻪ‬ ‫اي‬.‫ﻧﻤﻮﻧـﻪ‬ ‫در‬ ‫ﻣﻘـﺪار‬ ‫اﯾـﻦ‬‫ﻫـﺎي‬
‫ﻣﺤﺪ‬ ‫در‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬‫وده‬9/0‫اﺳـﺖ‬ ‫ﺑـﻮده‬ ‫ﺑﯿﺸـﺘﺮ‬ ‫ﺣﺘـﯽ‬ ‫و‬.
‫اﺳـﺘﻮاﻧﻪ‬ ‫از‬ ‫ﺑـﯿﺶ‬ ‫را‬ ‫ﻣﮑﻌﺒـﯽ‬ ‫ﺑـﺘﻦ‬ ‫ﻣﻘﺎوﻣﺖ‬ ،‫ﺟﺪاﺷﺪﮔﯽ‬‫اي‬
‫ﻣﯽ‬ ‫ﮐﺎﻫﺶ‬‫ﺳـﺮﯾﻊ‬ ‫ﺧﺮدﺷﺪﮔﯽ‬ ‫و‬ ‫ﺷﮑﻞ‬ ‫ﺗﻐﯿﯿﺮ‬ ‫زﯾﺮا‬ ‫دﻫﺪ؛‬‫ﺗـﺮ‬
‫ﺳﺒﺐ‬ ‫ﻓﺸﺎر‬ ‫دﺳﺘﮕﺎه‬ ‫زﯾﺮ‬ ‫در‬ ‫ﻣﮑﻌﺒﯽ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫در‬ ‫ﻗﺎﺋﻢ‬ ‫ﻻﯾﻪ‬ ‫ﯾﮏ‬
‫ﻣﯽ‬ ‫ﻣﮑﻌﺒﯽ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫ﺑﯿﺸﺘﺮ‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﮐﺎﻫﺶ‬‫ﺷﻮد‬.‫ﮐﻪ‬ ‫ﺣﺎﻟﯽ‬ ‫در‬
‫اﺳﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫در‬‫ﺿﻌﯿ‬ ‫ﻣﻨﻄﻘﻪ‬ ‫اﯾﻦ‬ ‫اي‬‫ﺗـﺄﺛﯿﺮ‬ ‫و‬ ‫ﺑﻮده‬ ‫اﻓﻘﯽ‬ ‫ﻒ‬
‫دارد‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﮐـﺎﻫﺶ‬ ‫ﺑـﺮ‬ ‫ﮐﻤﺘﺮي‬.‫ﭘـﺮ‬ ‫ﻻﯾـﻪ‬ ‫ﯾـﮏ‬ ‫وﺟـﻮد‬
‫ﺑﻪ‬ ‫ﻣﻘﺎوﻣﺖ‬‫دﺳﺖ‬‫ﭘﻮﺷﺶ‬ ‫ﻣﻮاد‬ ‫از‬ ‫آﻣﺪه‬‫ﮐـﻪ‬ ‫ﮐﻼﻫـﮏ‬ ‫دﻫﻨـﺪه‬
‫ﺳـﺒﮏ‬ ‫ﺑـﺘﻦ‬ ‫ﺑـﻪ‬ ‫ﻧﺴﺒﺖ‬ ‫ﺑﯿﺸﺘﺮي‬ ‫ﻣﻘﺎوﻣﺖ‬‫ﺑﺎﻋـﺚ‬ ،‫دارد‬ ‫داﻧـﻪ‬
‫اﺳﺘﻮاﻧﻪ‬ ‫آزﻣﻮﻧﻪ‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫اﻓﺰاﯾﺶ‬‫ﻣـﯽ‬ ‫اي‬‫ﺷـﻮد‬.‫اﺛـﺮ‬
‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﺑﺮ‬ ‫اﻧﺘﻬﺎﯾﯽ‬ ‫ﺷﺮاﯾﻂ‬‫ﻣﻌﻤـﻮﻟﯽ‬ ‫ﺑـﺘﻦ‬ ‫از‬ ‫ﮐﻤﺘـﺮ‬ ‫داﻧـﻪ‬
‫ا‬‫ﺳﺖ‬.‫ﭼﻨـﺪان‬ ‫ﻣﮑﻌﺒـﯽ‬ ‫ﻧﻤﻮﻧـﻪ‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫اﻓـﺰاﯾﺶ‬ ‫ﺑﻨﺎﺑﺮاﯾﻦ‬
‫ﭼﺸﻢ‬‫ﻧﯿﺴﺖ‬ ‫ﮔﯿﺮ‬.‫ﺑـﺘﻦ‬ ‫در‬ ‫ﮐﻪ‬ ‫داﻧﯿﻢ‬ ‫ﻣﯽ‬‫ﻣﻘﺎوﻣـﺖ‬ ‫ﭘـﺮ‬ ‫ﻫـﺎي‬
‫اﺳﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻧﺴﺒﺖ‬ ،‫ﻓﺸﺎري‬‫ﻣﮑﻌﺒﯽ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫ﺑﻪ‬ ‫اي‬
‫ﻣﯽ‬ ‫ﻧﺰدﯾﮏ‬ ‫ﯾﮏ‬ ‫ﻋﺪد‬ ‫ﺑﻪ‬‫ﺷﻮد‬.‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬‫ﺳﺒﮏ‬ ‫ﻫﺎي‬‫اﯾـﻦ‬ ‫داﻧﻪ‬
‫ﭘـﺲ‬ ‫اﺳـﺖ؛‬ ‫ﺑـﻮده‬ ‫ﮐـﻢ‬ ‫ﺳـﯿﻤﺎن‬ ‫ﺑـﻪ‬ ‫آب‬ ‫ﻧﺴـﺒﺖ‬ ،‫ﭘﮋوﻫﺶ‬
‫ﻧﺰدﯾ‬ ‫ﺧﺎﻃﺮ‬ ‫ﺑﻪ‬ ‫آن‬ ‫ﮔﺴﯿﺨﺘﮕﯽ‬‫ﺳﻨﮓ‬ ‫ارﺗﺠﺎﻋﯽ‬ ‫ﻣﺪول‬ ‫ﮑﯽ‬‫داﻧﻪ‬
‫ﺳـﻨﮓ‬ ‫و‬ ‫اﺳﺖ‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﭘﺮ‬ ‫ﺑﺘﻦ‬ ‫ﺷﺒﯿﻪ‬ ،‫ﺳﯿﻤﺎن‬ ‫ﺧﻤﯿﺮ‬ ‫و‬‫داﻧـﻪ‬
‫ـﯽ‬‫ـ‬‫ﻣ‬ ‫ـﺮد‬‫ـ‬‫ﺧ‬ ‫ـﺮ‬‫ـ‬‫زودﺗ‬ ‫آن‬‫ـﯿﻦ‬‫ـ‬‫ﺑ‬ ‫از‬ ‫ـﺮك‬‫ـ‬‫ﺗ‬ ‫ـﺎرﺗﯽ‬‫ـ‬‫ﻋﺒ‬ ‫ـﻪ‬‫ـ‬‫ﺑ‬ ‫و‬ ‫ـﻮد‬‫ـ‬‫ﺷ‬
‫ﺳﻨﮓ‬‫داﻧﻪ‬‫ﻣﯽ‬ ‫ﻋﺒﻮر‬ ‫ﻫﺎ‬‫ﺑـﻪ‬ ‫ﻧﺴﺒﺖ‬ ‫اﯾﻦ‬ ‫ﻧﺰدﯾﮑﯽ‬ ‫ﺑﻨﺎﺑﺮاﯾﻦ‬ ‫ﮐﻨﺪ؛‬
‫اﺳﺖ‬ ‫ﻣﻨﻄﻘﯽ‬ ‫ﯾﮏ‬.
‫رﯾﻠﻢ‬‫اﺳﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫در‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫ﻣﻌﺘﻘﺪ‬ ،‫ﺧﻮاص‬ ‫اﺛﺮ‬ ‫اي‬
‫ﺳﻨﮓ‬‫ﻓ‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﺮ‬ ‫درﺷﺖ‬ ‫داﻧﻪ‬‫ﻣﯽ‬ ‫ﮐﺎﻫﺶ‬ ‫ﺸﺎري‬‫ﯾﺎﺑﺪ‬]22[‫؛‬
‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫در‬ ‫ﭘﺲ‬‫ﺳﻨﮓ‬ ،‫داﻧﻪ‬‫در‬ ‫ﮐـﺎﻫﺶ‬ ‫اﺛـﺮ‬ ‫درﺷـﺖ‬ ‫داﻧﻪ‬
‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫و‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﺮرﺳﯽ‬-‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫داﻧﻪ‬‫ﭼﺎﻟﻪ‬ ‫ﻋﻠﯿﺮﺿﺎ‬ ‫و‬ ‫ﺧﺎﻧﺰادي‬ ‫ﻣﺼﻄﻔﯽ‬‫ﮐﺎﯾﯽ‬
84
‫دارد‬ ‫ﻣﻘﺎوﻣﺖ‬.‫اﺳـﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫در‬ ‫ﺗﺄﺛﯿﺮ‬ ‫اﯾﻦ‬‫از‬ ‫ﻧـﺎﭼﯿﺰﺗﺮ‬ ‫اي‬
‫ﻣﯽ‬ ‫ﻣﮑﻌﺒﯽ‬ ‫ﻧﻤﻮﻧﻪ‬‫ﻣﻘﺎوﻣﺖ‬ ‫و‬ ‫ﺷﻮد‬‫ﻧﻤﻮﻧـﻪ‬ ‫ﻧـﻮع‬ ‫دو‬ ‫اﯾﻦ‬ ‫ﻫﺎي‬
‫ﻣﯽ‬ ‫ﻧﺰدﯾﮑﺘﺮ‬ ‫ﯾﮑﺪﯾﮕﺮ‬ ‫ﺑﻪ‬‫ﺷﻮد‬.‫در‬ ‫ﻧﺴﺒﺖ‬ ‫اﯾﻦ‬ ‫دﯾﮕﺮ‬ ‫ﺳﻮي‬ ‫از‬
‫ﻧﻤﻮﻧﻪ‬‫ﮐﻤﺘ‬ ‫ﭼﻪ‬ ‫اﮔﺮ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬‫اﻣـﺎ‬ ‫ﺑـﻮده‬ ‫ﻟﯿﮑﺎ‬ ‫از‬ ‫ﺮ‬
‫اﺳﺖ‬ ‫ﻣﻌﻤﻮﻟﯽ‬ ‫ﺑﺘﻦ‬ ‫از‬ ‫ﺑﯿﺸﺘﺮ‬ ‫ﻫﻢ‬ ‫ﺑﺎز‬.‫ﻧﻈـﺮ‬ ‫ﺑـﻪ‬ ‫ﻣﻮرد‬ ‫اﯾﻦ‬ ‫در‬
‫ﻣﯽ‬‫ﻣﻌﻤـﻮﻟﯽ‬ ‫ﺑﺘﻦ‬ ‫ﺑﻪ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﺑﺘﻦ‬ ‫ﺧﺼﻮﺻﯿﺎت‬ ‫رﺳﺪ‬
‫ﻧﺰدﯾﮏ‬‫اﺳﺖ‬ ‫ﺗﺮ‬.
3-2-‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬
‫ﺳـﻦ‬ ‫در‬ ‫اﺳـﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴـﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫آزﻣﺎﯾﺶ‬28‫روي‬ ‫روز‬
‫ـﻪ‬‫ـ‬‫ﻧﻤﻮﻧ‬‫ـﺘﺎﻧﺪارد‬‫ـ‬‫اﺳ‬ ‫ـﺎي‬‫ـ‬‫ﻫ‬150×300‫ـﯽ‬‫ـ‬‫ﻣﯿﻠ‬‫ـﺎس‬‫ـ‬‫اﺳ‬ ‫ـﺮ‬‫ـ‬‫ﺑ‬ ‫و‬ ‫ـﺮ‬‫ـ‬‫ﻣﺘ‬
‫ﻣﺸﺨﺼﺎت‬ASTM‫ﺷﺪ‬ ‫اﻧﺠﺎم‬.‫ﺟﺪول‬ ‫در‬)3(‫آزﻣـﺎﯾﺶ‬ ‫ﻧﺘﺎﯾﺞ‬
‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬28،‫ﻣﺨﺼـﻮص‬ ‫وزن‬ ‫ﻫﻤﺮاه‬ ‫روزه‬
‫ﻣﯽ‬ ‫ﻣﺸﺎﻫﺪه‬ ‫ﺑﺘﻦ‬ ‫ﺑﺮﺷﯽ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﭘﻮاﺳﻮن‬ ‫ﺿﺮﯾﺐ‬‫ﮔﺮدد‬.
‫ﺟﺪول‬)4(‫راﯾﺞ‬ ‫از‬ ‫ﺑﺮﺧﯽ‬‫ﭘـﯿﺶ‬ ‫ﺑـﺮاي‬ ‫رواﺑﻂ‬ ‫ﺗﺮﯾﻦ‬‫ﺑﯿﻨـﯽ‬
‫ﻣﯽ‬ ‫ﻧﺸﺎن‬ ‫را‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬‫دﻫﺪ‬.‫ﺟـ‬ ‫در‬‫ﺪول‬)5(
‫ﺑﻪ‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﻧﺘﺎﯾﺞ‬‫دﺳﺖ‬‫ﺑـﺎ‬ ‫آزﻣﺎﯾﺸﻬﺎ‬ ‫از‬ ‫آﻣﺪه‬
‫ﺗﺨﻤﯿﻦ‬‫زده‬ ‫ﻫﺎي‬‫اﺳﺖ‬ ‫ﺷﺪه‬ ‫ﻣﻘﺎﯾﺴﻪ‬ ‫راﯾﺞ‬ ‫رواﺑﻂ‬ ‫ﺑﺎ‬ ‫ﺷﺪه‬.
‫ﻣﺪل‬ ‫از‬ ‫اﮔﺮ‬‫ﻣﺨﺼـﻮص‬ ‫وزن‬ ‫ﭘـﺎراﻣﺘﺮ‬ ‫ﮐـﻪ‬ ‫رﯾﺎﺿـﯽ‬ ‫ﻫﺎي‬
‫ﻧﺘـﺎﯾﺞ‬ ،‫ﺷـﻮد‬ ‫اﺳـﺘﻔﺎده‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﺮاي‬ ‫دارﻧﺪ‬
‫ﺑﻪ‬ ‫ﻣﺘﻔﺎوﺗﯽ‬‫ﻣﯽ‬ ‫دﺳﺖ‬‫آﯾﺪ‬.‫اراﺋـﻪ‬ ‫راﺑﻄﻪ‬ ‫اﮔﺮ‬‫در‬ ‫ﺷـﺪه‬ACI363
‫ﺑﻪ‬‫ﺑﻪ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﻧﺘﺎﯾﺞ‬ ‫رود‬ ‫ﮐﺎر‬‫آزﻣﺎﯾﺶ‬ ‫از‬ ‫آﻣﺪه‬ ‫دﺳﺖ‬
‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬‫ﻃـﺮح‬ ‫ﻫﻤـﮥ‬ ‫در‬ ‫ﻟﯿﮑﺎ‬ ‫و‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬‫از‬ ‫ﻫـﺎ‬
‫ﺑـﻪ‬ ‫ﻧﺘﺎﯾﺞ‬‫دﺳـﺖ‬‫ﮐﻮﭼـﮏ‬ ‫رﯾﺎﺿـﯽ‬ ‫ﻣـﺪل‬ ‫اﯾـﻦ‬ ‫از‬ ‫آﻣـﺪه‬‫و‬ ‫ﺗـﺮ‬
‫ﺑﻮد‬ ‫ﺧﻮاﻫﺪ‬ ‫ﻏﯿﺮﻣﻨﻄﻘﯽ‬.
‫اراﺋﻪ‬ ‫راﺑﻄﻪ‬‫در‬ ‫ﺷﺪه‬BS8110‫ﺑﻪ‬ ‫را‬ ‫ﻧﺘﺎﯾﺠﯽ‬‫ﻣـﯽ‬ ‫دﺳﺖ‬‫دﻫـﺪ‬
‫ﺗﺨﻤـ‬ ‫ﻧﺘـﺎﯾﺞ‬ ‫ﺑـﻮدن‬ ‫ﺑﯿﺸـﺘﺮ‬ ‫وﺟﻮد‬ ‫ﺑﺎ‬ ‫ﮐﻪ‬،‫واﻗﻌـﯽ‬ ‫ﻣﻘـﺎدﯾﺮ‬ ‫از‬ ‫ﯿﻦ‬
‫اﺳﺖ‬ ‫ﮐﻢ‬ ‫اﺧﺘﻼف‬.‫ﻧﻤﻮﻧﻪ‬ ‫ﺑﺮاي‬ ‫ﺣﺘﯽ‬ ‫ﻧﺘﺎﯾﺞ‬‫ﻟﯿﮑـﺎ‬ ‫ﺣـﺎوي‬ ‫ﻫـﺎي‬
‫ﻣﯽ‬ ‫ﻧﺰدﯾﮏ‬ ‫واﻗﻌﯿﺖ‬ ‫ﺑﻪ‬ ‫ﺑﯿﺸﺘﺮ‬‫ﺷﻮد‬.‫راﺑﻄﻪ‬‫ﻧﻮﯾﻞ‬‫ﻣﻘـﺎدﯾﺮي‬ ‫ﻧﯿـﺰ‬
‫اراﺋﻪ‬ ‫راﺑﻄﻪ‬ ‫ﺣﺪ‬ ‫در‬‫در‬ ‫ﺷﺪه‬BS8110‫ﻣﯽ‬ ‫ﺗﺨﻤﯿﻦ‬‫راﺑﻄﻪ‬ ‫اﻣﺎ‬ ‫زﻧﺪ؛‬
‫ﭘﺎﺋﯿﻦ‬ ‫ﺣﺪودي‬ ‫ﺗﺎ‬ ‫ﻣﻘﺎدﯾﺮي‬ ‫ﭘﻮﭘﻮوﯾﭻ‬‫رواﺑﻂ‬ ‫از‬ ‫ﺗﺮ‬‫اراﺋﻪ‬‫در‬ ‫ﺷـﺪه‬
BS8110‫ﻣﯽ‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﻧﻮﯾﻞ‬ ‫و‬‫زﻧﺪ‬.‫زده‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﻬﺘﺮﯾﻦ‬‫را‬ ‫ﺷـﺪه‬
‫ﻣﯽ‬‫رواﺑـﻂ‬ ‫از‬ ‫ﻣﯿـﺎﻧﮕﯿﻦ‬ ‫ﮔـﺮﻓﺘﻦ‬ ‫ﺑﺎ‬ ‫ﺗﻮان‬‫اراﺋـﻪ‬‫ﺷـﺪه‬BS8110‫و‬
‫ﺑﻪ‬ ‫ﭘﻮﭘﻮوﯾﭻ‬‫آورد‬ ‫دﺳﺖ‬.
‫ﺟﺪول‬)3(‫ﭘﻮآﺳﻮن‬ ‫ﺿﺮﯾﺐ‬ ،‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫آزﻣﺎﯾﺶ‬ ‫ﻧﺘﺎﯾﺞ‬
‫ﺑﺘﻦ‬ ‫ﺑﺮﺷﯽ‬ ‫ﻣﺪول‬ ‫و‬
‫ﻃﺮح‬ ‫ﻧﺎم‬
‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬
‫اﺳﺘﺎﺗﯿﮑﯽ‬(GPa)
‫ﺿﺮﯾﺐ‬
‫ﭘﻮاﺳﻮن‬
‫ﻣﺪول‬‫ﺑﺮﺷﯽ‬
(GPa)
L190/1419/026/6
L267/1518/064/6
L357/1819/080/7
S188/1620/070/5
S227/2122/044/7
S330/1922/089/6
‫ﺟﺪول‬)4(‫راﯾﺞ‬ ‫از‬ ‫ﺑﺮﺧﯽ‬‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﺮاي‬ ‫رواﺑﻂ‬ ‫ﺗﺮﯾﻦ‬
‫اﺳﺘﺎﺗﯿﮑﯽ‬
‫آﺋﯿﻦ‬‫ﻧﺎﻣﻪ‬
‫ﻣﺮﺑﻮط‬
‫ﻣﺪول‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﺮاي‬ ‫ﻣﻌﻤﻮل‬ ‫رواﺑﻂ‬
‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬
ACI-363R
0.5
s cE 3320f 6900 
‫ﻧﻮﯾﻞ‬-]23[0.5 1.5
s cE (3320f 6900)( )
2320

 
BS-8110 ]24[2 0.33 6
s cuE 1.7 f 10
  
‫ﭘﻮﭘﻮوﯾﭻ‬-]25[
2
3
s cuE 1.19f
‫ﺟﺪول‬)5(‫ﺗﺨﻤﯿﻦ‬‫زده‬ ‫ﻫﺎي‬‫ﺑﻪ‬ ‫ﺷﺪه‬‫راﯾﺞ‬ ‫رواﺑﻂ‬ ‫وﺳﯿﻠﮥ‬(GPa)
‫ﭘﯿﺶ‬‫ﻣﻌﺘﺒﺮ‬ ‫رواﺑﻂ‬ ‫ﺑﺮاﺳﺎس‬ ‫ﺑﯿﻨﯽ‬(MPa) ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬
‫ﺑﺪﺳﺖ‬‫آﻣﺪه‬
‫ﻧﺎم‬
‫ﻃﺮح‬ACI-363R ‫ﻧﻮﯾﻞ‬ BS-8110 ‫ﭘﻮﭘﻮوﯾﭻ‬
25/25 26/16 88/15 17/13 90/14 L1
19/26 98/17 82/17 07/14 67/15 L2
47/27 06/20 11/20 32/15 57/18 L3
63/27 37/22 89/23 47/15 88/16 S1
90/28 03/24 65/25 73/16 27/21 S2
05/30 66/25 27/27 90/17 30/19 S3
‫ﺳـﺒﮏ‬ ‫ﺧﺎص‬ ‫وﺿﻌﯿﺖ‬ ‫دﻟﯿﻞ‬ ‫ﺑﻪ‬ ‫اﺳﺖ‬ ‫ﻣﺴﻠﻢ‬‫ﻧـﻮع‬ ‫از‬ ‫داﻧـﻪ‬
‫ﺑـﺮاي‬ ‫ﺧـﺎص‬ ‫ﻣـﺪل‬ ‫ﯾـﮏ‬ ‫اراﺋـﻪ‬ ‫ﺑـﻪ‬ ‫ﻧﯿـﺎز‬ ،‫اﯾﺮان‬ ‫ﺗﻮﻟﯿﺪ‬ ‫ﻟﯿﮑﺎي‬
‫ﺑﺘﻦ‬‫ﻧﯿﻤﻪ‬ ‫ﻫﺎي‬‫ﺳﺒﮏ‬‫و‬ ‫ﭘﺮﻋﯿﺎر‬ ‫و‬ ‫ﮐﻢ‬ ‫ﺳﯿﻤﺎن‬ ‫ﺑﻪ‬ ‫آب‬ ‫ﻧﺴﺒﺖ‬ ‫ﺑﺎ‬ ‫داﻧﻪ‬
‫ﻣﯽ‬ ‫اﺣﺴﺎس‬ ‫آن‬ ‫ﺑﺪون‬ ‫ﯾﺎ‬ ‫ﺳﯿﻠﯿﺴﯽ‬ ‫دوده‬ ‫داراي‬‫ﺷﻮد‬.
‫ﻋﻠﻤﯽ‬ ‫ﻣﺠﻠﻪ‬-‫ﻣﺪرس‬ ‫ﻋﻤﺮان‬ ‫ﭘﮋوﻫﺸﯽ‬‫ﺷﻤﺎره‬ ،‫دوازدﻫﻢ‬ ‫دوره‬4/‫زﻣﺴﺘﺎن‬1391
85
‫ﺿﺮﯾﺐ‬ ‫ﺑﺮاي‬‫ﻣﯽ‬ ‫ﭘﯿﺸﻨﻬﺎد‬ ‫ﭘﻮاﺳﻮن‬‫ﻣﻘﺪار‬ ‫ﺷﻮد‬18/0‫ﺑـﺮاي‬
‫ﺑﺘﻦ‬‫و‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬22/0‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬‫اﺳـﮑﻮرﯾﺎ‬ ‫ﺣـﺎوي‬ ‫ﻫﺎي‬
‫ﺷﻮد‬ ‫ﻣﻨﻈﻮر‬.
‫ﻣـﺪول‬ ‫ﻣﻘﺪار‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬ ‫ﺑﺎ‬ ‫ﺑﺘﻮان‬ ‫ﮐﻪ‬ ‫اﯾﻦ‬ ‫ﺑﺮاي‬
‫ﺳﺎده‬ ‫را‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬‫ﻣـﺪل‬ ً‫ﻻ‬‫ﻣﻌﻤﻮ‬ ‫آورد‬ ‫ﺑﺪﺳﺖ‬ ‫ﺗﺮ‬‫ﻫـﺎﯾﯽ‬
‫ﻣﯽ‬ ‫اراﺋﻪ‬‫ﺷﻮد‬.‫ﻣﺪل‬‫ﺳﺎده‬ ‫رﯾﺎﺿﯽ‬ ‫ﻫﺎي‬‫ﻣﻮ‬ ‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬‫ﺟﻮد‬:
Es= 0.478 fc + 0.13 (R=0.95) )5(
Es= 0.255 fc + 7.942 (R=0.31) )6(
Es= 1.15×1.19×fc
0.66
(R=0.98) )7(
‫رواﺑﻂ‬5،6‫و‬ ‫اﺳﮑﻮرﯾﺎ‬ ،‫ﻟﯿﮑﺎ‬ ‫ﺑﻪ‬ ‫ﻣﺮﺑﻮط‬ ‫ﺗﺮﺗﯿﺐ‬ ‫ﺑﻪ‬7‫ﺑﻪ‬ ‫ﻣﺮﺑﻮط‬
‫اﺳﺖ‬ ‫دو‬ ‫ﻫﺮ‬.‫راﺑﻄـﻪ‬7‫اﻓﺰاﯾﻨـﺪه‬ ‫ﺿـﺮﯾﺐ‬15/1‫راﺑﻄـﻪ‬ ‫در‬ ‫را‬
‫اﺳـﺖ‬ ‫ﮐﺮده‬ ‫اﻋﻤﺎل‬ ‫ﭘﻮﭘﻮوﯾﭻ‬.‫ﻣـﺪل‬ ‫ﺳـﻪ‬‫اراﺋـﻪ‬‫ﺿـﺮﯾﺐ‬ ‫ﺷـﺪه‬
‫ـﺪ‬‫ـ‬‫ﻧﺪارﻧ‬ ‫ـﺎﻧﯽ‬‫ـ‬‫ﯾﮑﺴ‬ ‫ـﺘﮕﯽ‬‫ـ‬‫ﻫﻤﺒﺴ‬.‫ـﻪ‬‫ـ‬‫راﺑﻄ‬ ‫ـﺖ‬‫ـ‬‫ﺣﻘﯿﻘ‬ ‫در‬7‫ـﺮﯾﻦ‬‫ـ‬‫ﺑﻬﺘ‬
‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬ ‫را‬ ‫ﺗﺨﻤﯿﻦ‬‫اﺳﺖ‬ ‫داده‬ ‫اراﺋﻪ‬ ‫ﻣﻮﺟﻮد‬ ‫ﻫﺎي‬.
3-3-‫ﻣﻨﺤﻨﯽ‬‫ﺗﻨﺶ‬ ‫ﻫﺎي‬-‫ﮐﺮﻧﺶ‬
‫ﮔﻔﺘﻪ‬ ‫رواﺑﻂ‬ ‫از‬ ‫اﺳﺘﻔﺎده‬ ‫ﺑﺎ‬‫ﻣﻨﺤﻨـﯽ‬ ‫ﻣﻘﺪﻣـﻪ‬ ‫ﺑﺨﺶ‬ ‫در‬ ‫ﺷﺪه‬‫ﻫـﺎي‬
‫ﺗﻨﺶ‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫ﻧﺰدﯾﮏ‬ ‫ﮐﻪ‬ ‫ﺷﺪ‬ ‫زده‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﻫﺎ‬‫ﺗﺨﻤـﯿﻦ‬ ‫ﺗﺮﯾﻦ‬
‫ﻣﻨﺤﻨﯽ‬ ‫ﺑﻪ‬‫در‬ ‫واﻗﻌـﯽ‬ ‫ﻫﺎي‬‫ﺷـﮑﻞ‬‫ﻫـﺎي‬)1(‫و‬)2(‫ﺷـﺪه‬ ‫آورده‬
‫اﺳﺖ‬.‫ﻧﺰدﯾﮏ‬ ‫ﺣﺘﯽ‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫ﻣﺸﺨﺺ‬ ‫ﮐﺎﻣﻼ‬‫ﺗﺨﻤـﯿﻦ‬ ‫ﺗﺮﯾﻦ‬‫ﻫـﺎ‬
‫ﭼﺸـﻢ‬ ‫اﺧـﺘﻼف‬ ‫واﻗﻌﯽ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺑﺎ‬ ‫ﻧﯿﺰ‬‫ﻋـﻼوه‬ ‫ﺑـﻪ‬ ‫دارد؛‬ ‫ﮔﯿـﺮي‬
‫ﻣﻨﺤﻨﯽ‬‫اﺳـﺖ‬ ‫ﻧﺰدﯾـﮏ‬ ‫ﺧﯿﻠﯽ‬ ‫ﺧﻄﯽ‬ ‫ﺣﺎﻟﺖ‬ ‫ﺑﻪ‬ ‫واﻗﻌﯽ‬ ‫ﻫﺎي‬.‫ﺑـﺎ‬
‫ﺗـﻨﺶ‬ ‫راﺑﻄـﻪ‬ ‫ﻋﻤـﻮﻣﯽ‬ ‫روﻧﺪ‬ ‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬-‫ﺑـﺘﻦ‬ ‫در‬ ‫ﮐـﺮﻧﺶ‬‫ﻫـﺎي‬
‫ﻧﯿﻤﻪ‬‫ﺳﺒﮏ‬‫ﺗﻤﺎم‬ ‫و‬ ‫داﻧﻪ‬‫ﺳﺒﮏ‬‫ﺧﻄـﯽ‬ ‫و‬ ‫داﻧـﻪ‬‫ﺑـﻮد‬‫ﺑﺨـﺶ‬ ‫در‬ ‫آن‬ ‫ن‬
‫ﻋﻤﺪه‬‫ﻣﯽ‬ ‫ﻧﻈﺮ‬ ‫ﺑﻪ‬ ‫ﺻﻌﻮدي‬ ‫ﺷﺎﺧﻪ‬ ‫از‬ ‫اي‬‫ﮐـﺮد‬ ‫ﻗﺒـﻮل‬ ‫ﺑﺘﻮان‬ ‫رﺳﺪ‬
‫رﻓﺘـﺎر‬ ‫و‬ ‫اﻻﺳﺘﯿﺴـﯿﺘﻪ‬ ‫ﻣـﺪول‬ ‫ﻧﺰدﯾﮑﯽ‬ ‫ﺧﺎﻃﺮ‬ ‫ﺑﻪ‬ ‫ﺣﺎﻟﺖ‬ ‫اﯾﻦ‬ ‫ﮐﻪ‬
‫ﺳﺒﮏ‬ ‫و‬ ‫ﺳﯿﻤﺎن‬ ‫ﺧﻤﯿﺮ‬‫ﺑﻪ‬ ‫ﻟﯿﮑﺎ‬ ‫داﻧﻪ‬‫اﺳﺖ‬ ‫آﻣﺪه‬ ‫وﺟﻮد‬.‫ﺑـﺎ‬ ‫ﺷـﺎﯾﺪ‬
‫ﺣﺪ‬ ‫ﺑﺘﻮان‬ ‫ﺣﺎﻟﺖ‬ ‫اﯾﻦ‬ ‫وﺟﻮد‬35‫ﯾﺎ‬40‫ﻓﺸـﺎري‬ ‫ﺗـﻨﺶ‬ ‫درﺻـﺪ‬
‫ﺑ‬ ‫وﺗﺮي‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﺗﻌﯿﯿﻦ‬ ‫ﺑﺮاي‬ ‫ﮐﻪ‬ ‫ﻧﻬﺎﯾﯽ‬‫ﻪ‬‫ﻣـﯽ‬ ‫ﮐـﺎر‬‫رود‬
‫ﺑﻪ‬ ‫را‬75‫ﯾﺎ‬80‫رﺳﺎﻧﺪ‬ ‫درﺻﺪ‬.
3-3-1-‫ﻣﺪل‬‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫رﯾﺎﺿﯽ‬ ‫ﻫﺎي‬-‫ﮐﺮﻧﺶ‬
‫اﻟﻒ‬(‫ﺻﻌﻮدي‬ ‫ﺷﺎﺧﻪ‬
‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬ ‫ﺑﺎ‬‫ﺷﮑﻞ‬)3(‫ﻣﯽ‬ ‫ﻧﻈﺮ‬ ‫ﺑﻪ‬‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﻬﺘﺮﯾﻦ‬ ‫رﺳﺪ‬‫ﺑـﺮاي‬ ‫ﻫﺎ‬
‫ﺑﺘﻦ‬ ‫ﻣﺸﺨﺼﻪ‬ ‫ﻣﻨﺤﻨﯽ‬‫آزﻣﺎﯾﺶ‬ ‫ﻫﺎي‬‫ﻣـﺪول‬ ‫ﻣﺒﻨـﺎي‬ ‫ﺑـﺮ‬ ‫را‬ ‫ﺷـﺪه‬
‫ﺑﺘﻦ‬ ‫ﺳﮑﺎﻧﺖ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬‫ﻣﯽ‬ ‫ﻫﺎ‬‫ﺑﺘﻦ‬ ‫اﯾﻦ‬ ‫رﻓﺘﺎر‬ ‫و‬ ‫زد‬ ‫ﺗﻮان‬‫ﺑـﺮ‬ ‫ﻫـﺎ‬
‫ﺧﻼ‬‫ﺑﺘﻦ‬ ‫ف‬‫ﻣﻨﺤﻨـﯽ‬ ‫ﻧـﻮﻋﯽ‬ ‫از‬ ً‫ﻻ‬‫ﻣﻌﻤـﻮ‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫ﻣﻌﻤﻮﻟﯽ‬ ‫ﻫﺎي‬
‫ﻣﯽ‬ ‫ﺗﺒﻌﯿﺖ‬ ‫دوم‬ ‫درﺟﻪ‬‫ﮐﻨﻨﺪ‬.
‫ﺷﮑﻞ‬)1(‫ﻣﻨﺤﻨﯽ‬‫ﺗﻨﺶ‬ ‫ﻫﺎي‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬(L1)
‫ﺷﮑﻞ‬)2(‫ﻣﻨﺤﻨﯽ‬‫ﺗﻨﺶ‬ ‫ﻫﺎي‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬(S1)
‫ﻣـﺪول‬ ‫ﺑـﻪ‬ ‫ﺷـﺪه‬ ‫زده‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﯾﮏ‬ ‫درﺟﻪ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺷﯿﺐ‬ ‫ﻧﺴﺒﺖ‬
‫زﯾﺮ‬ ‫در‬ ‫ﺑﺘﻦ‬ ‫ﻫﺮ‬ ‫در‬ ‫ﺳﮑﺎﻧﺖ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬‫اﺳﺖ‬ ‫آﻣﺪه‬.
٠
۵
١٠
١۵
٢٠
٢۵
٣٠
٣۵
٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣
‫(ﺗﻨﺶ‬MPa)
‫ﮐﺮﻧﺶ‬
L1
TODESCHINI
٠
١٠
٢٠
٣٠
۴٠
۵٠
٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣
(‫ﺗﻨﺶ‬MPa)
‫ﮐﺮﻧﺶ‬
S1
HOGNESTAD
‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫و‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﺮرﺳﯽ‬-‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫داﻧﻪ‬‫ﭼﺎﻟﻪ‬ ‫ﻋﻠﯿﺮﺿﺎ‬ ‫و‬ ‫ﺧﺎﻧﺰادي‬ ‫ﻣﺼﻄﻔﯽ‬‫ﮐﺎﯾﯽ‬
86
‫ﺟﺪول‬)6(‫ﺗﺨﻤﯿﻦ‬ ‫ﯾﮏ‬ ‫درﺟﻪ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺷﯿﺐ‬‫زده‬‫ﺳﮑﺎﻧﺖ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﺑﻪ‬ ‫ﺷﺪه‬
‫ﻃﺮح‬ ‫ﻧﻮع‬‫ﺷﯿﺐ‬ ‫ﻧﺴﺒﺖ‬‫ﻣﺪول‬ ‫ﺑﻪ‬ ‫ﻣﻨﺤﻨﯽ‬
L1120/1
L2058/1
L3977/0
S1977/0
S1936/0
S1950/0
‫ﻣﺸﺎﻫﺪه‬ ‫ﺿﺮاﯾﺐ‬ ‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬ ‫ﺑﺎ‬‫ﺟﺪول‬ ‫در‬ ‫ﺷﺪه‬)6(‫ﻟﯿﮑـﺎ‬ ‫ﺑـﺮاي‬
‫ﻧﺴـﺒﺖ‬ ‫ﻣﻨﺤﻨـﯽ‬ ‫ﺷـﯿﺐ‬ ،‫ﺑـﺘﻦ‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫اﻓﺰاﯾﺶ‬ ‫ﺑﺎ‬‫ﻣـﺪول‬ ‫ﺑـﻪ‬
‫ﻣﯽ‬ ‫ﮐﺎﻫﺶ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬‫ﯾﺎﺑﺪ‬.‫ﺳـﻪ‬ ‫ﻫﺮ‬ ‫در‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺑﺎ‬ ‫راﺑﻄﻪ‬ ‫در‬
‫ﺑـﻪ‬ ‫ﮐـﻪ‬ ‫اﺳـﺖ‬ ‫ﻣـﺪول‬ ‫از‬ ‫ﮐﻤﺘـﺮ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺷﯿﺐ‬ ،‫اﺧﺘﻼط‬ ‫ﻃﺮح‬
‫داﻧـﻪ‬ ‫اﻻﺳﺘﯿﺴـﯿﺘﻪ‬ ‫ﻣـﺪول‬ ‫ﺑﻮدن‬ ‫ﺑﯿﺸﺘﺮ‬ ‫ﺧﺎﻃﺮ‬‫اﺳـﮑﻮرﯾﺎ‬ ‫ﻫـﺎي‬
‫اﺳﺖ‬ ‫ﻟﯿﮑﺎ‬ ‫ﺑﻪ‬ ‫ﻧﺴﺒﺖ‬.
‫ﺷﮑﻞ‬)3(‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺻﻌﻮدي‬ ‫ﻗﺴﻤﺖ‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫ﺳﺒﮏ‬ ‫ﻫﺎي‬‫داﻧﻪ‬
y = 16684x - 0.595
R² = 0.997
٠
١٠
٢٠
٣٠
۴٠
٠ ٠.٠٠٠۵ ٠.٠٠١ ٠.٠٠١۵ ٠.٠٠٢
L1
L1
Linear (L1)
y = 16487x + 1.623
R² = 0.997
٠
١٠
٢٠
٣٠
۴٠
۵٠
٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣
S1
S1
Linear (S1)
y = 16581x + 0.150
R² = 0.999
٠
١٠
٢٠
٣٠
۴٠
٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣
L2
L2
Linear (L2)
y = 19896x + 0.818
R² = 0.999
٠
١٠
٢٠
٣٠
۴٠
۵٠
٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣
S2
S2
Linear (S2)
y = 18135x + 0.718
R² = 0.997
٠
١٠
٢٠
٣٠
۴٠
۵٠
٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣
L3
L٣
Linear (L ٣(
y = 18347x + 1.002
R² = 0.997
٠
١٠
٢٠
٣٠
۴٠
۵٠
۶٠
٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣
S3
S3
Linear (S3)
Linear (S3)
‫ﻋﻠﻤﯽ‬ ‫ﻣﺠﻠﻪ‬-‫ﻣﺪرس‬ ‫ﻋﻤﺮان‬ ‫ﭘﮋوﻫﺸﯽ‬‫ﺷﻤﺎره‬ ،‫دوازدﻫﻢ‬ ‫دوره‬4/‫زﻣﺴﺘﺎن‬1391
87
‫ب‬(‫ﻧﺰوﻟﯽ‬ ‫ﺷﺎﺧﻪ‬
‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬ ‫ﺑﺎ‬‫ﺷﮑﻞ‬)4(‫ﻣـﯽ‬ ‫ﺗﻈـﺮ‬ ‫ﺑﻪ‬‫ﻣﺸﺨﺼـﯽ‬ ‫راﺑﻄـﻪ‬ ‫رﺳـﺪ‬
‫ﻧﻤﯽ‬‫ﺑﺠـﺰ‬ ‫اﻣـﺎ‬ ‫داد؛‬ ‫ﭘﯿﺸـﻨﻬﺎد‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﻧﺰوﻟﯽ‬ ‫ﺷﺎﺧﻪ‬ ‫ﺑﺮاي‬ ‫ﺗﻮان‬
‫ﺑﺘﻦ‬L1‫ﻣﻨﺤﻨـﯽ‬ ‫ﺷـﮑﻞ‬ ‫ﺑـﻪ‬ ‫ﺗﻘﺮﯾـﺐ‬ ‫ﺑـﺎ‬ ‫آن‬ ‫ﻧﺰوﻟﯽ‬ ‫ﺷﺎﺧﻪ‬ ‫ﮐﻪ‬
،‫دارد‬ ‫ﺧﻄـﯽ‬ ‫ﻣﻨﺤﻨـﯽ‬ ‫ﺑـﻪ‬ ‫ﻧﺴﺒﺖ‬ ‫ﺑﻬﺘﺮي‬ ‫ﻫﻤﺒﺴﺘﮕﯽ‬ ‫دو‬ ‫درﺟﻪ‬
‫ﺑﺘﻦ‬ ‫ﺑﺎﻗﯽ‬‫ﺷـ‬ ‫ﺑـﺎ‬ ‫ﻫـﺎ‬‫و‬ ‫ﺻـﻌﻮدي‬ ‫ﺷـﺎﺧﻪ‬ ‫از‬ ‫ﮐﻤﺘـﺮ‬ ‫ﻣﻨﻔـﯽ‬ ‫ﯿﺐ‬
‫ﺑﻪ‬‫اﺳـﺖ‬ ‫ﺧﻄـﯽ‬ ‫ﺻﻮرت‬.‫ﺗـﻨﺶ‬ ‫ﺑﯿﺸـﯿﻨﻪ‬ ‫ﺑـﺎ‬ ‫ﻣﺘﻨـﺎﻇﺮ‬ ‫ﮐـﺮﻧﺶ‬
‫ﺛﺒﺖ‬‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬ ‫ﻣﻨﺤﻨﯽ‬ ‫در‬ ‫ﺷﺪه‬‫ﺣﺪود‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬2000
‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬ ‫و‬ ‫ﻣﯿﮑﺮوﮐﺮﻧﺶ‬‫ﺣﺪود‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬2500
‫اﺳﺖ‬ ‫ﺑﻮده‬ ‫ﻣﯿﮑﺮوﮐﺮﻧﺶ‬.
‫ﺷﮑﻞ‬)4(‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﻧﺰوﻟﯽ‬ ‫ﻗﺴﻤﺖ‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫ﺳﺒﮏ‬ ‫ﻫﺎي‬‫داﻧﻪ‬
y = -8518x + 48.43
R² = 0.982
y = -2E+06x2 + 4415.x + 31.52
R² = 0.996
٠
۵
١٠
١۵
٢٠
٢۵
٣٠
٣۵
٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ٠.٠٠۴
L1 L1
Linear (L1)
Poly. (L1)
y = -13861x + 72.95
R² = 0.999
٠
١٠
٢٠
٣٠
۴٠
۵٠
٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ٠.٠٠۴
S1
S١
Linear (S١(
y = -11865x + 59.55
R² = 0.995
٠
١٠
٢٠
٣٠
۴٠
٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ٠.٠٠۴
L2
L2
Linear (L2)
y = -16438x + 83.67
R² = 0.998
٠
١٠
٢٠
٣٠
۴٠
۵٠
٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ٠.٠٠۴
S2
S2
Linear (S2)
y = -13762x + 72.62
R² = 0.998
٠
١٠
٢٠
٣٠
۴٠
۵٠
٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ٠.٠٠۴
L3
L3
Linear (L3)
y = -14880x + 90.11
R² = 0.996
٠
١٠
٢٠
٣٠
۴٠
۵٠
۶٠
٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ٠.٠٠۴
S3
Series1
Linear (S3)
‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫و‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﺮرﺳﯽ‬-‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫داﻧﻪ‬‫ﭼﺎﻟﻪ‬ ‫ﻋﻠﯿﺮﺿﺎ‬ ‫و‬ ‫ﺧﺎﻧﺰادي‬ ‫ﻣﺼﻄﻔﯽ‬‫ﮐﺎﯾﯽ‬
88
4-‫ﻧﺘﯿﺠﻪ‬‫ﮔﯿﺮي‬
‫ﺑﺮرﺳﯽ‬ ‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬ ‫ﺑﺎ‬‫ﺗﺤﻠﯿﻞ‬ ‫و‬ ‫ﺗﺠﺰﯾﻪ‬ ‫و‬ ‫آزﻣﺎﯾﺸﮕﺎﻫﯽ‬ ‫ﻫﺎي‬‫ﻫـﺎي‬
‫اﻧﺠﺎم‬‫ﻣﯽ‬ ‫ﺷﺪه‬‫ﻧﺘﯿﺠﻪ‬ ‫ﺗﻮان‬‫ﮔﯿﺮي‬‫ﻧﻤﻮد‬ ‫ﻣﻄﺮح‬ ‫را‬ ‫زﯾﺮ‬ ‫ﻧﻬﺎﯾﯽ‬ ‫ﻫﺎي‬:
1.‫ﻋﯿـﺎر‬ ‫ﺑـﺎ‬ ‫ﺳﯿﻤﺎﻧﯽ‬ ‫ﻣﻮاد‬ ‫از‬ ‫اﺳﺘﻔﺎده‬ ‫ﺑﺎ‬Kg/m3
500‫ﻧﺴـﺒﺖ‬ ‫و‬
‫ﺳﯿﻤﺎن‬ ‫ﺑﻪ‬ ‫آب‬30/0‫ﻣﯿـﺰان‬ ‫ﺑـﻪ‬ ‫ﺳﯿﻠﯿﺴﯽ‬ ‫دوده‬ ‫ﺟﺎﯾﮕﺰﯾﻨﯽ‬ ،10
‫اﻧـﺪازه‬ ‫ﺑﯿﺸـﯿﻨﮥ‬ ‫ﺑـﺎ‬ ‫ﻟﯿﮑﺎ‬ ،‫ﺳﯿﻤﺎن‬ ‫وزن‬ ‫درﺻﺪ‬5/12‫ﻣﺘـﺮ‬ ‫ﻣﯿﻠـﯽ‬
)10-3(‫ﻧﻮع‬ ‫ﭘﺮﺗﻠﻨﺪ‬ ‫ﺳﯿﻤﺎن‬ ،‫ﻣﻌﻤﻮﻟﯽ‬ ‫ﻣﺎﺳﻪ‬ ،1‫ﻓﻮق‬ ،‫روان‬‫ﮐﻨﻨﺪه‬
‫ﻣﯿﺰان‬ ‫ﺑﻪ‬1‫ﻣﻘﺎوﻣـﺖ‬ ‫ﺑﯿﺸـﺘﺮﯾﻦ‬ ،‫ﺳـﯿﻤﺎﻧﯽ‬ ‫ﻣـﻮاد‬ ‫وزن‬ ‫درﺻـﺪ‬
‫ﻓﺸﺎري‬28‫ﺑﺘﻦ‬ ‫ﺑﯿﻦ‬ ‫روزه‬‫ﺳﺒﮏ‬ ‫ﻫﺎي‬‫ﻣﺮ‬ ،‫داﻧﻪ‬‫ﻣﺨﻠـﻮط‬ ‫ﺑـﻪ‬ ‫ﺑﻮط‬
S3‫ﺑﺮاﺑـﺮ‬ ‫ﻣﮑﻌﺒـﯽ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫ﺑﺮاي‬ ‫ﮐﻪ‬ ‫ﺑﻮده‬MPa63/54‫ﺑـﺮاي‬ ‫و‬
‫اﺳﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬‫ﺑﺮاﺑﺮ‬ ‫اي‬MPa62/48‫اﺳـﺖ‬.‫ﻣﻘﺎوﻣـﺖ‬ ‫ﮐﻤﺘـﺮﯾﻦ‬
‫ﻓﺸﺎري‬28‫ﻣﺨﻠﻮط‬ ‫ﺑﻪ‬ ‫ﻣﺮﺑﻮط‬ ‫روزه‬L1‫ﻧﻤﻮﻧـﻪ‬ ‫ﺑﺮاي‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬
‫ﺑﺮاﺑﺮ‬ ‫ﻣﮑﻌﺒﯽ‬MPa2/33‫اﺳـﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫ﺑﺮاي‬ ‫و‬‫ﺑﺮاﺑـﺮ‬ ‫اي‬MPa
54/30‫اﺳﺖ‬.‫ﺑﺘﻦ‬ ‫وزن‬ ‫ﮐﺎﻫﺶ‬‫ﻟﯿﮑـﺎ‬ ‫ﺣـﺎوي‬ ‫ﻫﺎي‬‫ﺣـﺪود‬30
‫ﺑﺘﻦ‬ ‫و‬ ‫درﺻﺪ‬‫ﺣـﺪود‬ ‫اﺳـﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬20‫ﺑـﻮد‬ ‫درﺻـﺪ‬.
‫ﻣﻘﺎوﻣﺖ‬ ‫ﻧﺘﺎﯾﺞ‬‫ﻓﺸﺎري‬ ‫ﻫﺎي‬28‫آزﻣﻮﻧﻪ‬ ‫وزن‬ ‫ﺗﺎﺑﻊ‬ ً‫ﻼ‬‫ﻋﻤ‬ ‫روزه‬‫ﻫﺎ‬
‫ﻣﯽ‬ ‫ﮐﺎﻫﺶ‬ ‫ﻧﯿﺰ‬ ‫ﻣﻘﺎوﻣﺖ‬ ،‫آن‬ ‫ﮐﺎﻫﺶ‬ ‫ﺑﺎ‬ ‫و‬ ‫اﺳﺖ‬‫ﯾﺎﺑﺪ‬.
2.‫ﺑﺘﻦ‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬‫ﺗﻮﺟـﻪ‬ ‫ﺑﺎ‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬
‫داﻧﻪ‬ ‫ﺑﺎﻓﺖ‬ ‫ﺑﻪ‬‫ﺣﺪود‬ ‫ﺑﯿﻦ‬ ‫ﺑﻨﺪي‬15‫ﺗﺎ‬19‫ﺑﻮد‬ ‫ﮔﯿﮕﺎﭘﺎﺳﮑﺎل‬.‫اﯾﻦ‬
‫ﺑـﺘﻦ‬ ‫ﺑﺮاي‬ ‫ﻣﻘﺪار‬‫ﺑـﯿﻦ‬ ‫اﺳـﮑﻮرﯾﺎ‬ ‫ﺣـﺎوي‬ ‫ﻫـﺎي‬17‫ﺗـﺎ‬50/19
‫ﺑﻮد‬ ‫ﮔﯿﮕﺎﭘﺎﺳﮑﺎل‬.‫اﻻﺳﺘﯿﺴـﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﺮاي‬ ‫ﻧﯿﺰ‬ ‫رواﺑﻄﯽ‬
‫ﺑـﺘﻦ‬ ‫اﯾﻦ‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬‫وزن‬ ‫و‬ ‫ﻓﺸـﺎري‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫اﺳـﺎس‬ ‫ﺑـﺮ‬ ‫ﻫـﺎ‬
‫اﺳﺖ‬ ‫ﺷﺪه‬ ‫اراﺋﻪ‬ ‫ﻣﺨﺼﻮﺻﺸﺎن‬.
3.‫ﭘﻮاﺳﻮن‬ ‫ﺿﺮاﯾﺐ‬‫ﺑﺘﻦ‬‫ﻃـﻮر‬ ‫ﺑﻪ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬
‫ﻣﺘﻮﺳﻂ‬19/0‫و‬22/0‫ﺷﺪ‬ ‫ﺗﻌﯿﯿﻦ‬.
4.‫ﻧﺴ‬‫ﻧﻤﻮﻧﻪ‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺒﺖ‬‫اﺳـﺘﻮاﻧﻪ‬ ‫ﺑـﻪ‬ ‫ﻣﮑﻌﺒﯽ‬ ‫ﻫﺎي‬‫اي‬
‫ﺑﺘﻦ‬ ‫در‬‫از‬ ‫ﮐﻤﺘﺮ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬1‫ﻣﺤـﺪوده‬ ‫در‬ ‫و‬
92/0‫ﺗﺎ‬89/0‫ﺷﺪ‬ ‫ﺛﺒﺖ‬.
5.‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫ﻣﻄﺎﻟﻌﻪ‬ ‫ﻫﺎي‬‫ﺷـﺎﺧﻪ‬ ‫در‬ ‫ﺷﺪه‬‫ﻫـﺎي‬
‫اﺳﺖ‬ ‫ﺑﻮده‬ ‫ﻣﻨﻔﯽ‬ ً‫ﺎ‬‫ﺗﻘﺮﯾﺒ‬ ،‫ﻧﺰوﻟﯽ‬ ‫و‬ ‫ﺻﻌﻮدي‬.‫ﺗﻮﺻـﯿﻪ‬‫ﻧﯿـﺰ‬ ‫ﻫـﺎﯾﯽ‬
‫ﻣﻨﺤﻨﯽ‬ ‫اﯾﻦ‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﺮاي‬‫ﺷﺪ‬ ‫اراﺋﻪ‬ ‫ﻫﺎ‬.
5-‫ﻣﺮاﺟﻊ‬
[1] Topcu I.B., "Semi-lightweight concretes
produced by volcanic slags", Cem Concr Res
27(1) (1997) 15-21
[2] Al-Khaiat H., Haque M.N., "Effect of initial
curing on early strength and physical properties
of lightweight concrete", Cem Concr Res 28(6)
(1998) 859-866
[3] Ke Y., Beacour A.L., Ortola S., Dumontets H.,
Cabrillac R., "Influence of volume fraction and
characteristics of lightweight aggregates on the
mechanical properties of concrete", Cons Build
Mat 23 (2009) 2821-2828
]4[،‫ﻣﺤﺴـﻦ‬ ،‫ﺗﺪﯾﻦ‬"‫و‬ ‫ﺑﺮرﺳـﯽ‬‫ارزﯾـﺎﺑﯽ‬،‫ﮐﺸﺸـﯽ‬ ‫ﻣﻘﺎوﻣـﺖ‬
‫ﺑـﺘﻦ‬ ‫ﺧﻮردﮔﯽ‬ ‫ﺷﺪت‬ ‫و‬ ‫ﭘﻮاﺳﻮن‬ ‫ﺿﺮﯾﺐ‬ ،‫ارﺗﺠﺎﻋﯽ‬ ‫ﻣﺪول‬
‫ﭘﺮ‬ ‫ﺳﺒﮏ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫ﻣﺼﺎﻟﺢ‬ ‫ﺑﺎ‬ ‫ﻣﻘﺎوﻣﺖ‬"‫ﭘﺎﯾـﺎن‬ ،‫ﻧﺎﻣـﻪ‬
،‫اﯾـﺮان‬ ‫ﺻـﻨﻌﺖ‬ ‫و‬ ‫ﻋﻠﻢ‬ ‫داﻧﺸﮕﺎه‬ ،‫ﻋﻤﺮان‬ ‫داﻧﺸﮑﺪه‬ ،‫دﮐﺘﺮي‬
‫ﺷﻬﺮﯾﻮر‬1381.
[5] Demirboga R., Orung I., Gul R., "Effects of
expanded perlite aggregate and mineral
admixtures on the compressive strength of low-
density concretes". Cement Concrete Res. 31(11)
(2001) 1627-1632
[6] Chen H.J., Yen T., Lia T.P., Huang Y.L.,
"Determination of dividing strength and it's
relation to the concrete strength in lightweight
aggregate concrete", Cement and Concrete
Composition,Vol. 21, (1999) 29-37
[7] European Union-Brite Euram III, "Definitions
and international consensus report, BE96-
3942/R1", 1998
[8] Zhang M.H., Gjorv O.E., "Characteristics of
lightweight aggregates for high-strength
concrete", ACI Mater. J., 1991(March-April)
150-158
[9] Yang C.C., Huang R., "Approximate strength of
lightweight aggregate using micromechanics
‫ﻋﻠﻤﯽ‬ ‫ﻣﺠﻠﻪ‬-‫ﻣﺪرس‬ ‫ﻋﻤﺮان‬ ‫ﭘﮋوﻫﺸﯽ‬‫ﺷﻤﺎره‬ ،‫دوازدﻫﻢ‬ ‫دوره‬4/‫زﻣﺴﺘﺎن‬1391
89
method", Adv. Cem. Based Mater., 7(3-4) (1998)
133-138
[10] Wasserman R., Bentur A., "Effect of
lightweight fly ash aggregate microstructure on
the strength of concretes", Cem. Concr. Res.,
27(4) (1997) 525-537
[11] Kilic A., Atis C.D., Yasar E., Ozcan F., "High-
strength lightweight concrete made with scoria
aggregate containing mineral admixtures", Cem
Concr Res, 33 (2003) 1595-1599
[12] Macgregor J.G., "Reinforced concrete
mechanics and design", Prentice Hall, 3rd
Edition, 1997
[13] Hognestad E., "A study of combined bending
and axial load in reinforced concrete members",
Bulletin 399, University of Illinois Engineering
Experiment Station, Urbana, I11., November
1951, 128
[14] Todeschini C.E., Bianchini A.C., and Clyde E.
Kesler, "Behavior of concrete columns
reinforced with high strength steels", ACI
Journal, Proceedings. Vol. 61, No. 6, June 1964,
701-716
[15] Popovics S., "A numerical approach to the
complete stress-strain curve of concrete",
Cement and Concrete Research, Vol. 3, (1973)
583-599
[16] Yi S.T., Kim J.K., Oh T.K., "Effect of strength
and age on the stress-strain curves of concrete
specimens", Cement and Concrete Research,
Vol. 33, (2003) 1235-1244
[17] Blechman I., "Stage model of stress-strain
relationship for concrete under short-term load –
Part.1", Cement and Concrete Research, Vol.
18, (1988) 863-873
[18] ASTM C330-99, "Standard specification for
lightweight aggregates for structural concrete",
American Society for Testing And Materials,
March 1999
[19] ASTM C150-99a, "Standard specification for
portland cement", American Society For Testing
And Materials, November 1999
[20] ASTM C 494/C 494M – 99a, "Standard
specification for chemical admixtures for
concrete", American Society For Testing And
Materials, December 1999
[21] ACI 211.2-98, "Standard practice for selecting
proportions for structural lightweight concrete",
American Concrete Institute, 1998
]22[،‫ﻫﺮﻣﺰ‬ ،‫ﻓﺎﻣﯿﻠﯽ‬"‫ﺑﺘﻦ‬ ‫ﺧﻮاص‬"‫ﭼـﺎپ‬ ،‫ﺑﯿﺮوﻧﯽ‬ ‫اﺑﻮرﯾﺤﺎن‬ ،
،‫اول‬1378
[23] Neville A.M., "Properties of concrete",
Longman, 3rd Edition, 1981
[24] Slate F.O., Nilson A.H., Martinez S.,
"Mechanical properties of high strength
lightweight concrete", ACI Materials Journal,
Vol.3, (1986) 606-613
[25] Popovics S., "Strength and related properties of
concrete, a quantitative approach", JohnWiley,
1998

Weitere ähnliche Inhalte

Andere mochten auch

Inspirational
InspirationalInspirational
InspirationalDarla4229
 
Bangla Slide Share 2
Bangla Slide Share 2Bangla Slide Share 2
Bangla Slide Share 2Cambriannews
 
Mercedes C Class Cabriolet, S Class Cabriolet India Launch - Press Release
Mercedes C Class Cabriolet, S Class Cabriolet India Launch - Press ReleaseMercedes C Class Cabriolet, S Class Cabriolet India Launch - Press Release
Mercedes C Class Cabriolet, S Class Cabriolet India Launch - Press ReleaseRushLane
 
The necessity to integration of value engineering and risk management in cons...
The necessity to integration of value engineering and risk management in cons...The necessity to integration of value engineering and risk management in cons...
The necessity to integration of value engineering and risk management in cons...Alireza Chalekaee
 
Guía de números cuánticos
Guía  de  números  cuánticosGuía  de  números  cuánticos
Guía de números cuánticosGiuliana Tinoco
 

Andere mochten auch (9)

Inspirational
InspirationalInspirational
Inspirational
 
Bangla Slide Share 2
Bangla Slide Share 2Bangla Slide Share 2
Bangla Slide Share 2
 
Mercedes C Class Cabriolet, S Class Cabriolet India Launch - Press Release
Mercedes C Class Cabriolet, S Class Cabriolet India Launch - Press ReleaseMercedes C Class Cabriolet, S Class Cabriolet India Launch - Press Release
Mercedes C Class Cabriolet, S Class Cabriolet India Launch - Press Release
 
The necessity to integration of value engineering and risk management in cons...
The necessity to integration of value engineering and risk management in cons...The necessity to integration of value engineering and risk management in cons...
The necessity to integration of value engineering and risk management in cons...
 
Rolling bearing
Rolling bearingRolling bearing
Rolling bearing
 
Pathopart2
Pathopart2Pathopart2
Pathopart2
 
Pathopart6
Pathopart6Pathopart6
Pathopart6
 
Guía de números cuánticos
Guía  de  números  cuánticosGuía  de  números  cuánticos
Guía de números cuánticos
 
Cell Structure And Function
Cell Structure And FunctionCell Structure And Function
Cell Structure And Function
 

MJCE18551364931000

  • 1. 79 ‫ﻋﻠﻤﯽ‬ ‫ﻣﺠﻠﻪ‬-‫ﭘﮋوﻫﺸﯽ‬ »‫ﻣــﺪرس‬ ‫ﻋﻤـﺮان‬« ‫دوره‬‫دوازدﻫﻢ‬‫ﺷﻤﺎره‬ ،4،‫زﻣﺴﺘﺎن‬1391 ‫ﺗﺤﻘﯿﻘﺎﺗﯽ‬ ‫ﯾﺎدداﺷﺖ‬: ‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫و‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﺮرﺳﯽ‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬ ‫ﺳﺒﮏ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫داﻧﻪ‬ ‫ﺧﺎﻧﺰادي‬ ‫ﻣﺼﻄﻔﯽ‬1* ‫ﻋﻠﯿﺮﺿﺎ‬ ،‫ﭼﺎﻟﻪ‬‫ﮐﺎﯾﯽ‬2 1-‫اﯾﺮان‬ ‫ﺻﻨﻌﺖ‬ ‫و‬ ‫ﻋﻠﻢ‬ ‫داﻧﺸﮕﺎه‬ ،‫ﻋﻤﺮان‬ ‫داﻧﺸﮑﺪه‬ ،‫اﺳﺘﺎدﯾﺎر‬ 2-‫اﯾﺮان‬ ‫ﺻﻨﻌﺖ‬ ‫و‬ ‫ﻋﻠﻢ‬ ‫داﻧﺸﮕﺎه‬ ،‫ﻋﻤﺮان‬ ‫داﻧﺸﮑﺪه‬ ،‫ارﺷﺪ‬ ‫ﮐﺎرﺷﻨﺎس‬ khanzadi@iust.ac.ir ‫درﯾﺎﻓﺖ‬ ‫ﺗﺎرﯾﺦ‬:07/10/1390‫ﭘﺬﯾﺮش‬ ‫ﺗﺎرﯾﺦ‬:20/12/1390 ‫ﭼﮑﯿﺪه‬-‫ا‬ ‫در‬‫ﯾ‬‫ﻦ‬‫ﭘﮋوﻫﺶ‬‫ﺳﻨﮕﺪاﻧﻪ‬ ‫از‬ ‫اﺳﺘﻔﺎده‬ ‫اﻣﮑﺎن‬‫ﻫﺎ‬‫ي‬‫اﺳﮑﻮر‬‫ﯾ‬‫ﺎ‬‫ﻟ‬ ‫و‬‫ﯿ‬‫ﮑﺎ‬‫ي‬‫ﺑ‬ ‫ﮐﺸﻮر‬ ‫در‬ ‫ﻣﻮﺟﻮد‬‫ﺮاي‬‫ﺗﻮﻟ‬‫ﯿ‬‫ﺪ‬‫ﺳـﺒﮏ‬ ‫ﺑـﺘﻦ‬‫ﭘﺮﻣﻘﺎوﻣـﺖ‬ ‫داﻧـﻪ‬ ‫ﺑﺮرﺳ‬‫ﯽ‬‫اﺳﺖ‬ ‫ﺷﺪه‬.‫ﻃﺮح‬ ‫ﺑﺮاﺳﺎس‬‫ﻫﺎ‬‫ي‬‫ﮔﻮﻧﺎﮔﻮن‬‫اﺧﺘﻼط‬‫و‬‫روش‬‫ﻫﺎ‬‫ي‬‫ﺗﻮﻟ‬ ،‫ﻣﺮﺳﻮم‬‫ﯿ‬‫ﺪ‬‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬‫داﻧـﻪ‬‫ا‬‫ي‬‫ﻓﺸـﺎر‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﺑـﺎ‬‫ي‬28‫روزه‬‫ي‬ ‫ﺑ‬‫ﯿ‬‫ﺸﺘﺮ‬‫از‬40‫آن‬ ‫ﺑﺘﻮان‬ ‫ﮐﻪ‬ ‫ﻣﮕﺎﭘﺎﺳﮑﺎل‬‫ﺑ‬ ‫در‬ ‫را‬‫ﺘﻦ‬‫ﺑ‬ ‫ﻣﺴﻠﺢ‬‫ﻪ‬‫ﮐ‬‫ﺷﺪ‬ ‫ﻣﻤﮑﻦ‬ ،‫ﺑﺮد‬ ‫ﺎر‬.‫ﺑ‬‫ﺮاي‬‫ﺑﺮرﺳ‬‫ﯽ‬‫ﻣﮑـﺎﻧ‬ ‫ﻣﺸﺨﺼﺎت‬‫ﯿ‬‫ﮑ‬‫ﯽ‬‫ﮐﻮﺗـﺎه‬‫ا‬ ‫ﻣـﺪت‬‫ﯾـ‬‫ﻦ‬‫ﺑـﺘﻦ‬، ‫آزﻣﺎ‬‫ﯾ‬‫ﺶ‬‫ﻫﺎ‬‫ي‬‫ﻣﺨﺘﻠﻔ‬‫ﯽ‬‫ﻓﺸﺎر‬ ‫ﻣﻘﺎوﻣﺖ‬ ،‫ﺑﺘﻦ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﭼﻮن‬‫ي‬،‫اﻻﺳﺘ‬ ‫ﻣﺪول‬‫ﯿ‬‫ﺴ‬‫ﯿ‬‫ﺘﻪ‬‫اﺳﺘﺎﺗ‬‫ﯿ‬‫ﮑ‬‫ﯽ‬‫ﺿﺮ‬ ‫و‬‫ﯾ‬‫ﺐ‬‫ﺷﺪ‬ ‫اﻧﺠﺎم‬ ‫ﭘﻮاﺳﻮن‬‫؛‬‫رواﺑﻄ‬‫ﯽ‬‫ﻧ‬‫ﯿـ‬‫ﺰ‬ ‫ﺑﺮاي‬‫ﭘ‬‫ﯿ‬‫ﺶ‬‫ﺑ‬‫ﯿ‬‫ﻨ‬‫ﯽ‬‫اﻻﺳﺘ‬ ‫ﻣﺪول‬‫ﯿ‬‫ﺴ‬‫ﯿ‬‫ﺘﻪ‬‫اﺳﺘﺎﺗ‬‫ﯿ‬‫ﮑ‬‫ﯽ‬‫ا‬‫ﯾ‬‫ﻦ‬‫ﺑﺘﻦ‬‫ﻫﺎ‬‫ﻣﺨﺼﻮﺻﺸﺎن‬ ‫وزن‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﺮاﺳﺎس‬‫ﺳﻦ‬ ‫در‬28‫اﺳـﺖ‬ ‫ﺷـﺪه‬ ‫اراﺋﻪ‬ ‫روز‬. ‫ﻣﺸﺨﺺ‬‫ﺷ‬‫ﺑ‬ ‫ﺑﺘﻦ‬ ‫وزن‬ ‫اﻓﺰاﯾﺶ‬ ‫ﺑﺎ‬ ‫ﮐﻪ‬ ‫ﺪ‬‫ﺎ‬‫داﻧﻪ‬ ‫ﺑﺎﻓﺖ‬ ‫در‬ ‫ﺗﻐﯿﯿﺮ‬‫ﺑـﺘﻦ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ،‫ﺑﻨﺪي‬‫آزﻣـﺎﯾﺶ‬ ‫ﻫـﺎي‬،‫ﺷـﺪه‬‫اﻓـﺰاﯾﺶ‬ ‫اﺳﺖ‬ ‫ﯾﺎﻓﺘﻪ‬.‫ﺑﺘﻦ‬ ‫اﯾﻦ‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﻬﺒﻮد‬ ‫در‬ ‫ﻧﯿﺰ‬ ‫ﺳﯿﻠﯿﺴﯽ‬ ‫دوده‬ ‫از‬ ‫اﺳﺘﻔﺎده‬‫ﺑﻮ‬ ‫ﻣﺆﺛﺮ‬ ‫ﻫﺎ‬‫اﺳﺖ‬ ‫ده‬.‫ﻣﯽ‬ ‫ﻧﺸﺎن‬ ‫ﻧﺘﺎﯾﺞ‬‫ﻟﯿﮑـﺎ‬ ‫و‬ ‫اﺳـﮑﻮرﯾﺎ‬ ‫ﮐﻪ‬ ‫دﻫﻨﺪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﻬﺒﻮد‬ ‫در‬‫ﺑﻮده‬ ‫ﻣﺆﺛﺮ‬ ‫ﻫﺎ‬‫ﻣﻨﺎﺳـﺐ‬ ‫ﻧﺘﺎﯾﺞ‬ ‫ﺑﻪ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﮐﻪ‬‫اﺳـﺖ‬ ‫رﺳـﯿﺪه‬ ‫ﺗـﺮي‬.‫ﺗـﻨﺶ‬ ‫ﻣﻨﺤﻨـﯽ‬-‫ﺑـﺘﻦ‬ ‫ﮐـﺮﻧﺶ‬‫ﻫـﺎي‬ ‫ﻣﻄﺎﻟﻌﻪ‬‫ﺗﻮﺻﯿﻪ‬ ‫و‬ ‫ﺷﺪ‬ ‫ﺑﺮرﺳﯽ‬ ‫ﺷﺪه‬‫ﻣﻨﺤﻨﯽ‬ ‫اﯾﻦ‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﺮاي‬ ‫ﻫﺎﯾﯽ‬‫ﺷﺪ‬ ‫اراﺋﻪ‬ ‫ﻫﺎ‬.‫ﻣﻨﺤﻨﯽ‬ ،‫ﻧﺘﺎﯾﺞ‬ ‫اﺳﺎس‬ ‫ﺑﺮ‬‫ﺷﺎﺧﻪ‬ ‫در‬ ‫ﻫﺎ‬‫ﻫـﺎي‬‫ﻧﺰوﻟـﯽ‬ ‫و‬ ‫ﺻـﻌﻮدي‬ ‫ﺑﻮدﻧﺪ‬ ‫ﺧﻄﯽ‬ ً‫ﺎ‬‫ﺗﻘﺮﯾﺒ‬. ‫واژﮔﺎن‬‫ﮐﻠﯿﺪ‬‫ي‬:‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ،‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ،‫اﺳﮑﻮرﯾﺎ‬ ،‫ﻟﯿﮑﺎ‬ ،‫داﻧﻪ‬-‫ﮐﺮﻧﺶ‬ 1-‫ﻣﻘﺪﻣﻪ‬ ‫ﺑـﺎ‬ ‫ﺳﺒﮏ‬ ‫ﻣﺼﺎﻟﺢ‬ ‫ﺑﺮاي‬ ‫ﺗﻘﺎﺿﺎ‬ ‫و‬ ‫ﯾﺎﻓﺘﻪ‬ ‫اﻓﺰاﯾﺶ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﺗﻮﻟﯿﺪ‬ ‫ﻫـﻢ‬ ‫ﺳـﺎز‬ ‫و‬ ‫ﺳـﺎﺧﺖ‬ ‫ﺑـﺮاي‬ ‫ﻗﺒـﻮل‬ ‫ﻗﺎﺑﻞ‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﻣﯽ‬ ‫اﻓﺰاﯾﺶ‬‫ﯾﺎﺑﺪ‬.‫ﺑـﺘﻦ‬ ‫از‬ ،‫ﺑـﺘﻦ‬ ‫ﻣﺨﺘﻠﻒ‬ ‫اﻧﻮاع‬ ‫ﺷﺎﻣﻞ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮐﻢ‬‫ﺑﻠﻮك‬ ‫ﺗﻮﻟﯿﺪ‬ ‫در‬ ‫ﺑﯿﺸﺘﺮ‬ ‫ﮐﻪ‬ ‫ﻣﻘﺎوﻣﺖ‬‫ﻏﯿﺮﺳﺎزه‬ ‫ﻫﺎي‬‫ﺑـﻪ‬ ‫اي‬‫ﮐـﺎر‬ ‫ﻣﯽ‬‫ﺑﺘﻦ‬ ‫ﺗﺎ‬ ‫رود‬‫ﺳﺎزه‬ ‫ﻫﺎي‬‫از‬ ‫ﺑـﯿﺶ‬ ‫ﻓﺸـﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﺎ‬ ‫اي‬100 ‫ﻣﯽ‬ ‫ﻣﮕﺎﭘﺎﺳﮑﺎل‬‫ﺷﻮد‬.‫ﺑﺴﯿﺎري‬ ‫ﻣﺤﻘﻘﯿﻦ‬]3-1[‫ﺗﺤﻘﯿﻘﺎﺗﺸﺎن‬ ‫در‬ ‫آورده‬‫ﺳﺒﮏ‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫ﻫﻮاي‬ ‫ﺣﻔﺮات‬ ‫ﺧﺎﻃﺮ‬ ‫ﺑﻪ‬ ‫ﮐﻪ‬ ‫اﻧﺪ‬‫داﻧﻪ‬،‫ﻫـﺎ‬ ‫ﻣﻘﺎوﻣـﺖ‬ ،‫وزن‬ ‫ﺑـﻪ‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﺑـﺎﻻي‬ ‫ﻧﺴـﺒﺖ‬ ‫داراي‬ ‫ﺑـﺘﻦ‬ ‫اﯾﻦ‬ ‫وﯾﮋﮔﯽ‬ ‫و‬ ‫ﭘﺎﯾﯿﻦ‬ ‫ﺣﺮارﺗﯽ‬ ‫اﻧﺒﺴﺎط‬ ‫ﺿﺮﯾﺐ‬ ،‫ﻣﻨﺎﺳﺐ‬ ‫ﮐﺸﺸﯽ‬‫ﻫﺎي‬ ‫دارد‬ ‫را‬ ‫ﺻﺪا‬ ‫و‬ ‫ﮔﺮﻣﺎ‬ ‫ﻣﻘﺎﺑﻞ‬ ‫در‬ ‫ﺑﻮدن‬ ‫ﻋﺎﯾﻖ‬ ‫ﺑﺮﺗﺮ‬.‫ﺑﺮ‬ ‫اﻓﺰون‬،‫اﯾﻦ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫در‬‫ﺳـﺎزه‬ ‫اﻋﻀﺎي‬ ‫ﻋﺮﺿﯽ‬ ‫ﻣﻘﻄﻊ‬ ،‫ﺗﺮ‬‫ﮐﻮﭼـﮏ‬ ‫اي‬‫ﺗـﺮ‬ ‫ﻣﯽ‬‫اﻗﺘﺼﺎدي‬ ‫اﺟﺮا‬ ‫و‬ ‫ﺷﻮد‬‫ﺷﺪ‬ ‫ﺧﻮاﻫﺪ‬ ‫ﺗﺮ‬. ‫ﺳـﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﻫﺮ‬ ‫ﺗﻮﻟﯿﺪ‬‫ﺑـﻮدن‬ ‫دﺳـﺘﺮس‬ ‫در‬ ‫ﺑـﻪ‬ ً‫ﻼ‬‫ﮐـﺎﻣ‬ ‫داﻧـﻪ‬
  • 2. ‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫و‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﺮرﺳﯽ‬-‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫داﻧﻪ‬‫ﭼﺎﻟﻪ‬ ‫ﻋﻠﯿﺮﺿﺎ‬ ‫و‬ ‫ﺧﺎﻧﺰادي‬ ‫ﻣﺼﻄﻔﯽ‬‫ﮐﺎﯾﯽ‬ 80 ‫ﺳﺒﮏ‬‫داﻧـﻪ‬‫اﺳـﺖ‬ ‫ﻣـﺮﺗﺒﻂ‬ ‫ﻫـﺎ‬]4.[‫ﻣﺤﻘﻘـﯿﻦ‬ ‫ﺑﺮﺧـﯽ‬]4،3[‫در‬ ‫ﺑﺘﻦ‬ ‫روي‬ ‫ﺗﺤﻘﯿﻘﺎﺗﺸﺎن‬‫ﺳﺒﮏ‬ ‫ﻫﺎي‬‫ﺳـﺒﮏ‬ ‫ﺣﺎوي‬ ‫داﻧﻪ‬‫داﻧـﻪ‬‫ﻫـﺎي‬ ‫ﺗﻮف‬ ‫ﭼﻮن‬ ‫ﻃﺒﯿﻌﯽ‬1 ‫ﭘﺮﻟﯿﺖ‬ ‫و‬2 ‫ﺳـﺒﮏ‬ ‫ﯾﺎ‬‫داﻧـﻪ‬‫ﻣﺼـﻨﻮﻋﯽ‬ ‫ﻫـﺎي‬ ‫ﻣﻨﺒﺴﻂ‬ ‫رس‬ ‫ﭼﻮن‬‫ﺷﻞ‬ ‫ﯾﺎ‬ ‫ﺷﺪه‬3 ‫ﮐﺮده‬ ‫ﻣﻄﺎﻟﻌﻪ‬‫اﻧﺪ‬.‫آن‬‫اﯾـﻦ‬ ‫ﺑـﻪ‬ ‫ﻫﺎ‬ ‫رﺳﯿﺪه‬ ‫ﻧﺘﯿﺠﻪ‬‫اﻓﺰودﻧـﯽ‬ ‫ﮐـﻪ‬ ‫اﻧـﺪ‬،‫ﺑـﺎدي‬ ‫ﺧﺎﮐﺴـﺘﺮ‬ ‫ﻣﺎﻧﻨـﺪ‬ ‫ﻫـﺎﯾﯽ‬ ‫ﭘﻮزوﻻن‬ ‫و‬ ‫ﻣﯿﮑﺮوﺳﯿﻠﯿﺲ‬‫ﺳـﺒﺐ‬ ،‫ﺳـﺒﮏ‬ ‫ﺑـﺘﻦ‬ ‫در‬ ‫ﻃﺒﯿﻌﯽ‬ ‫ﻫﺎي‬ ‫ـﯽ‬‫ـ‬‫ﻣ‬ ‫ـﺘﻦ‬‫ـ‬‫ﺑ‬ ‫در‬ ‫ـﯽ‬‫ـ‬‫ﻣﺨﺘﻠﻔ‬ ‫ـﺎت‬‫ـ‬‫ﻣﺸﺨﺼ‬ ‫ـﻮد‬‫ـ‬‫ﺑﻬﺒ‬‫ـﻪ‬‫ـ‬‫ﮐ‬ ‫ـﺮا‬‫ـ‬‫ﭼ‬ ‫ـﻮد؛‬‫ـ‬‫ﺷ‬ ‫واﮐﻨﺶ‬‫ﻣﺸﺨﺼـﺎ‬ ‫ﺑﻬﺒـﻮد‬ ‫ﺑﻪ‬ ‫ﻣﻨﺠﺮ‬ ‫ﭘﻮزوﻻﻧﯽ‬ ‫ﻫﺎي‬‫ﻣﮑـﺎﻧﯿﮑﯽ‬ ‫ت‬ ‫ﻣﯽ‬‫ﺷﻮد‬]5[.‫ﺳـﺎزه‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫در‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬،‫اي‬21‫ﺗـﺎ‬ 28‫اﺳﺖ‬ ‫ﻣﮕﺎﭘﺎﺳﮑﺎل‬]6[‫ﻣـﻮاد‬ ‫ﺑـﻪ‬ ‫آب‬ ‫ﻧﺴـﺒﺖ‬ ‫ﮐﺎﻫﺶ‬ ‫ﺑﺎ‬ ‫ﮐﻪ‬ ،‫ذرات‬ ‫ـﺪازه‬‫ـ‬‫اﻧ‬ ‫ـﯿﻨﮥ‬‫ـ‬‫ﺑﯿﺸ‬ ‫ـﺎﻫﺶ‬‫ـ‬‫ﮐ‬ ،‫ـﯿﻤﺎن‬‫ـ‬‫ﺳ‬ ‫ـﺰاﯾﺶ‬‫ـ‬‫اﻓ‬ ،‫ـﺒﻨﺪه‬‫ـ‬‫ﭼﺴ‬ ‫ﺳـﺒﮏ‬ ‫ﻣﺎﺳﻪ‬ ‫ﺟﺎﯾﮕﺰﯾﻨﯽ‬‫از‬ ‫اﺳـﺘﻔﺎده‬ ‫و‬ ‫ﻃﺒﯿﻌـﯽ‬ ‫ﻣﺎﺳـﻪ‬ ‫ﺑـﺎ‬ ‫داﻧـﻪ‬ ‫اﻓﺰودﻧﯽ‬‫ﻣﯽ‬ ‫اﻓﺰاﯾﺶ‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫اﯾﻦ‬ ‫ﻫﺎ‬‫ﯾﺎﺑﺪ‬. ‫ﺿﻌﯿﻒ‬‫ﺟﺰ‬ ‫ﺗﺮﯾﻦ‬‫ﻣﻨﻄﻘـﻪ‬ ‫ﯾـﺎ‬ ‫ﺳـﯿﻤﺎن‬ ‫ﻣﺎﺗﺮﯾﺲ‬ ،‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ء‬ ‫ﺗﻤﺎﺳﯽ‬4 ‫ﺳـﺒﮏ‬ ‫ﺑﻠﮑـﻪ‬ ،‫ﻧﯿﺴـﺖ‬‫اﺳـﺖ‬ ‫داﻧـﻪ‬.‫دﻟﯿـﻞ‬ ‫ﻫﻤـﯿﻦ‬ ‫ﺑـﻪ‬ ‫ﺳﯿﻤﺎن‬ ‫ﻣﺎﺗﺮﯾﺲ‬ ‫ﮐﯿﻔﯿﺖ‬ ‫ﺑﺎ‬ ‫ﺗﻨﻬﺎ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﻧﻤــﯽ‬ ‫ﺳــﻨﺠﯿﺪه‬ ‫آن‬‫ﺳــﺒﮏ‬ ‫ﻣﺸﺨﺼــﺎت‬ ‫و‬ ‫ﺷــﻮد‬‫ﺣﺠــﻢ‬ ‫داﻧــﻪ‬ ‫ﺳﺒﮏ‬‫داﻧﻪ‬‫ﺳﺒﮏ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫و‬ ‫ﺑﺘﻦ‬ ‫در‬ ‫ﻫﺎ‬‫ﻣـﻮرد‬ ‫اﯾﻦ‬ ‫در‬ ‫ﻧﯿﺰ‬ ‫داﻧﻪ‬ ‫ﻣﻮﺛﺮﻧﺪ‬]7،3[. ‫ﺟﻮرو‬ ‫و‬ ‫ژاﻧﮓ‬]8[‫ﺗﺎﺛﯿﺮ‬‫ﻣﻘﺎوﻣـﺖ‬ ‫ﺑـﺮ‬ ‫ﺳـﺒﮏ‬ ‫ﺑـﺘﻦ‬ ‫ﭼﮕﺎﻟﯽ‬ ‫ﺑﺮرﺳﯽ‬ ‫را‬ ‫ﭘﺮﻣﻘﺎوﻣﺖ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮔﺴﯿﺨﺘﮕﯽ‬ ‫ﺳﺎزوﮐﺎر‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﮐﺮده‬‫اﻧﺪ‬.‫ﺳـﺒﮏ‬ ‫ﮐـﻢ‬ ‫ﺣﺠـﻢ‬ ‫اﻫﻤﯿـﺖ‬ ‫ﺑﺴﯿﺎري‬ ‫ﻣﺤﻘﻘﯿﻦ‬‫در‬ ‫داﻧـﻪ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬‫ﺑـﺎ‬ ‫ﺗﻨﻬـﺎ‬ ‫را‬ ‫داﻧـﻪ‬ ‫ﭼﮕﺎﻟﯽ‬‫ﻣﯽ‬ ‫ﺷﺎن‬‫ﻣﮑـﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼـﺎت‬ ‫ﺳﻨﺠﺶ‬ ‫ﮐﻪ‬ ‫ﭼﺮا‬ ‫ﺳﻨﺠﻨﺪ؛‬ ‫ﺳﺒﮏ‬‫داﻧﻪ‬‫اﺳﺖ‬ ‫دﺷﻮار‬ ‫ﻫﺎ‬]3‫و‬9[.‫و‬‫ﺑﻨﺘـﻮر‬ ‫و‬ ‫اﺳﺮﻣﻦ‬]10[‫ﻧﺸـﺎن‬ ‫داده‬‫ﺳـﻨﮕﺪاﻧﻪ‬ ‫ﯾﮑﺴﺎن‬ ‫ﭼﮕﺎﻟﯽ‬ ‫ﮐﻪ‬ ‫اﻧﺪ‬‫اﯾﺠـﺎد‬ ‫ﺳـﺒﺐ‬ ً‫ﻻ‬‫ﻣﻌﻤـﻮ‬ ‫ﻫـﺎ‬ ‫ﻧﻤﯽ‬ ‫ﺑﺘﻦ‬ ‫در‬ ‫ﯾﮑﺴﺎن‬ ‫ﻣﻘﺎوﻣﺖ‬‫ﺷﻮد‬. ‫روش‬ ‫ﺑﺎ‬ ‫را‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬‫ﻣﯽ‬ ‫ﺗﻮﻟﯿﺪ‬ ‫ﻣﺨﺘﻠﻔﯽ‬ ‫ﻫﺎي‬‫ﮐﻨﻨـﺪ‬.‫ﺑـﺮاي‬ 1- tuff 2- perlite 3- shale 4- interfacial transition zone ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫داﺷﺘﻦ‬‫ﺳﺎزه‬ ‫داﻧﻪ‬‫ﺳﺒﮏ‬ ،‫ﭘﺮﻣﻘﺎوﻣﺖ‬ ‫و‬ ‫اي‬‫داﻧـﻪ‬‫ﺑـﻪ‬ ‫ﻫـﺎ‬ ‫ﺳﻨﮓ‬ ‫از‬ ‫ﺑﺨﺸﯽ‬ ‫ﺟﺎﯾﮕﺰﯾﻦ‬ ‫ﻋﻨﻮان‬‫داﻧﻪ‬‫ﻫﻤـ‬ ‫ﯾﺎ‬ ‫ﻣﻌﻤﻮﻟﯽ‬ ‫ﻫﺎي‬‫آن‬ ‫ﻪ‬ ‫ﻣﯽ‬ ‫ﮐﺎر‬ ‫ﺑﻪ‬‫رود‬.‫ﺳﺒﮏ‬ ‫ﮐﻠﯽ‬ ‫ﻃﻮر‬ ‫ﺑﻪ‬‫داﻧﻪ‬‫و‬ ‫ﻃﺒﯿﻌـﯽ‬ ‫ﻧﻮع‬ ‫دو‬ ‫ﺑﻪ‬ ‫ﻫﺎ‬ ‫ﻣـﯽ‬ ‫ﺗﻘﺴـﯿﻢ‬ ‫ﻣﺼﻨﻮﻋﯽ‬‫ﺷـﻮﻧﺪ‬.‫ﺳـﺒﮏ‬‫از‬ ‫ﭘـﺲ‬ ‫را‬ ‫ﻃﺒﯿﻌـﯽ‬ ‫داﻧـﻪ‬ ‫داﻧﻪ‬ ً‫ﺎ‬‫ﻣﺴﺘﻘﯿﻤ‬ ،‫ﻣﻌﺪن‬ ‫از‬ ‫اﺳﺘﺨﺮاج‬‫ﺑـﻪ‬ ‫ﺑﺘﻦ‬ ‫در‬ ‫و‬ ‫ﮐﺮده‬ ‫ﺑﻨﺪي‬‫ﮐـﺎر‬ ‫ﻣﯽ‬‫ﺑﺮﻧﺪ‬.‫راﯾﺞ‬ ‫از‬ ‫ﯾﮑﯽ‬‫ﺳﺒﮏ‬ ‫ﺗﺮﯾﻦ‬‫داﻧﻪ‬‫در‬ ‫ﻣﻮﺟـﻮد‬ ‫ﻃﺒﯿﻌﯽ‬ ‫ﻫﺎي‬ ‫اﯾﺮان‬"‫اﺳﮑﻮرﯾﺎ‬"‫ﺑﺎ‬ ‫ﻋﺎم‬ ‫زﺑﺎن‬ ‫در‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬‫ﻋﻨﻮان‬"‫ﭘـﺎ‬ ‫ﺳﻨﮓ‬" ‫ﻣﯽ‬ ‫ﺷﻨﺎﺧﺘﻪ‬‫ﺷﻮد‬.‫ﭘﻮﮐﻪ‬ ‫ﺟﺰء‬ ‫و‬ ‫دارد‬ ‫آذرﯾﻦ‬ ‫ﻣﻨﺸﺄ‬ ‫اﺳﮑﻮرﯾﺎ‬‫ﻫﺎي‬ ‫اﺳﺖ‬ ‫ﻣﻌﺪﻧﯽ‬.‫ﮐﻮه‬ ‫دﻫﺎﻧﻪ‬ ‫در‬ ‫ﺑﯿﺸﺘﺮ‬ ‫ﺳﻨﮓ‬ ‫اﯾﻦ‬‫آﺗﺸﻔﺸـﺎﻧﯽ‬ ‫ﻫﺎي‬ ‫ﮔﺪازه‬ ‫از‬ ‫و‬‫دارﻧـﺪ‬ ‫ﮐﻤـﯽ‬ ‫ﺳـﯿﻠﯿﺲ‬ ‫ﮐـﻪ‬ ‫ﻣﺬاﺑﯽ‬ ‫ﻫﺎي‬)‫ﺑﺎزاﻟـﺖ‬5 ( ‫ﻣﯽ‬ ‫اﯾﺠﺎد‬‫ﺷﻮد‬.‫ﻣﯽ‬ ‫و‬ ‫اﺳﺖ‬ ‫ﺗﯿﺮه‬ ‫آن‬ ‫رﻧﮓ‬‫رﻧـﮓ‬ ‫ﺑـﻪ‬ ‫ﺗﻮاﻧﺪ‬‫ﻫـﺎي‬ ‫ﻗﻬﻮه‬‫ﺧﺎﮐﺴـﺘﺮ‬ ،‫ﻗﺮﻣـﺰ‬ ،‫ﻗﺮﻣﺰ‬ ‫ﺑﻪ‬ ‫ﻣﺎﯾﻞ‬ ‫اي‬‫ﺑﺎﺷـﺪ‬ ‫ﺳـﯿﺎه‬ ‫ﯾـﺎ‬ ‫و‬ ‫ي‬. ‫ﺳﻨﮓ‬ ‫اﯾﻦ‬ ‫ﺑﯿﺸﺘﺮ‬‫دارﻧﺪ‬ ‫ﯾﮏ‬ ‫از‬ ‫ﺑﯿﺸﺘﺮ‬ ‫ﻣﺨﺼﻮﺻﯽ‬ ‫وزن‬ ‫ﻫﺎ‬]11[. ‫ﺳـﺎزه‬ ‫اﻋﻀـﺎي‬ ‫ﺗﻮﻟﯿـﺪ‬ ‫در‬ ‫ﭼﻨﺪاﻧﯽ‬ ‫ﮐﺎرﺑﺮد‬ ‫ﻣﺎده‬ ‫اﯾﻦ‬ ‫ﺗﺎﮐﻨﻮن‬‫اي‬ ‫اﺳـﮑﻮرﯾﺎ‬ ‫از‬ ‫اﺳﺘﻔﺎده‬ ‫ﻣﻮرد‬ ‫در‬ ‫ﮐﻤﯽ‬ ‫ﺗﺤﻘﯿﻘﺎت‬ ‫و‬ ‫اﺳﺖ‬ ‫ﻧﺪاﺷﺘﻪ‬ ‫اﺳـﺖ‬ ‫ﺷﺪه‬ ‫اﻧﺠﺎم‬ ‫ﭘﺮﻣﻘﺎوﻣﺖ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫در‬.‫اﺳـﮑﻮرﯾﺎ‬ ‫ﻣﻌـﺎدن‬ ‫ﺗﻮﺟﻪ‬ ‫ﻗﺎﺑﻞ‬ ‫ﮐﺸﻮر‬ ‫ﻏﺮب‬ ‫ﺷﻤﺎل‬ ‫و‬ ‫ﻏﺮب‬ ‫در‬‫اﺳﺖ‬. ‫ﺳﺒﮏ‬ ‫ﺟﻤﻠﻪ‬ ‫از‬‫داﻧﻪ‬‫ﻣﻨﺒﺴﻂ‬ ‫رس‬ ،‫ﻣﺼﻨﻮﻋﯽ‬ ‫ﻫﺎي‬‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫ﺷﺪه‬ ‫ﻣـﯽ‬ ‫ﻧﺎﻣﯿـﺪه‬ ‫ﻟﯿﮑﺎ‬ ‫اﻏﻠﺐ‬‫ﺷـﻮد‬.،‫ﻟﯿﮑـﺎ‬ ‫ﺑـﺎ‬ ‫ﻣﺨﺘﻠـﻒ‬ ‫ﮐﺸـﻮرﻫﺎي‬ ‫در‬ ‫ﺑﺘﻦ‬‫ﺗﻤﺎم‬ ‫ﻫﺎي‬‫ﺳﺒﮏ‬‫ﻧﯿﻤﻪ‬ ‫ﯾﺎ‬ ‫داﻧﻪ‬‫ﺳﺒﮏ‬‫ﺳﺎزه‬ ‫داﻧﻪ‬‫ﻣﯽ‬ ‫را‬ ‫اي‬‫ﺳـﺎزﻧﺪ‬.‫در‬ ‫ﻣﯽ‬ ‫ﺗﻮﻟﯿﺪ‬ ‫ﺳﺒﮑﯽ‬ ‫ﻟﯿﮑﺎي‬ ‫ﻣﺎ‬ ‫ﮐﺸﻮر‬‫ﺳـﺎﺧﺖ‬ ‫ﺑـﺮاي‬ ً‫ﻻ‬‫ﻣﻌﻤﻮ‬ ‫ﮐﻪ‬ ‫ﺷﻮد‬ ‫ﺑﺘﻦ‬‫ﺷﯿﺐ‬ ،‫ﭘﺮﮐﻨﻨﺪه‬ ‫ﻫﺎي‬‫ﺑﺎم‬ ‫ﺑﻨﺪي‬‫و‬ ‫ﻫﺎ‬‫ﺑﻠـﻮك‬ ‫ﺳﺎﺧﺖ‬‫ﺳـﺒﮏ‬ ‫ﻫـﺎي‬ ‫ـﺎزه‬‫ـ‬‫ﺳ‬ ‫ﻧﯿﻤـﻪ‬ ‫ـﺎرﺑﺮد‬‫ـ‬‫ﮐ‬ ‫ﮐـﻪ‬‫ﻣـﯽ‬ ‫ـﺘﻔﺎده‬‫ـ‬‫اﺳ‬ ،‫دارد‬ ‫اي‬‫ـﻮد‬‫ـ‬‫ﺷ‬.‫ـﺎت‬‫ـ‬‫ﺗﺤﻘﯿﻘ‬ ‫ﺑﺘﻦ‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺗﻌﯿﯿﻦ‬ ‫در‬ ‫ﺳﻌﯽ‬ ‫ﻣﺨﺘﻠﻔﯽ‬‫ﺑﺎ‬ ‫ﺷﺪه‬ ‫ﺳﺎﺧﺘﻪ‬ ‫ﻫﺎي‬ ‫اﺳﺖ‬ ‫داﺷﺘﻪ‬ ‫ﻣﺨﺘﻠﻒ‬ ‫ﺷﺮاﯾﻂ‬ ‫در‬ ‫را‬ ‫اﯾﺮان‬ ‫ﻟﯿﮑﺎي‬. ‫ﻣﺸﺨﺺ‬‫ﺗـﻨﺶ‬ ‫ﻣﻨﺤﻨـﯽ‬ ‫ﺗﺨﻤـﯿﻦ‬ ‫ﺑﺮاي‬ ‫ﮐﻪ‬ ‫رواﺑﻄﯽ‬ ‫ﺗﺮﯾﻦ‬- ‫ﺷـﮑﻞ‬ ‫در‬ ‫ﺷﺪه‬ ‫اراﺋﻪ‬ ‫ﮐﺮﻧﺶ‬)1(‫اﺳـﺖ‬ ‫ﺷـﺪه‬ ‫آورده‬.‫ﻣﻨﺤﻨـﯽ‬ ‫ﺗ‬‫ﻮدﭼﯿﻨﯽ‬‫ﺗﺤﻠﯿﻠـﯽ‬ ‫ﻣﻄﺎﻟﻌـﺎت‬ ‫ﺑـﺮاي‬ ،‫آن‬ ‫ﭘﯿﻮﺳـﺘﻪ‬ ‫ﺗﺎﺑﻊ‬ ‫دﻟﯿﻞ‬ ‫ﺑﻪ‬ ‫اﺳﺖ‬ ‫ﻣﻨﺎﺳﺐ‬]12[. 5- basalt
  • 3. ‫ﺷﻤﺎره‬ ،‫دوازدﻫﻢ‬ ‫دوره‬4/‫زﻣﺴﺘﺎن‬1391 ‫ﮐﻮﺗﺎه‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫از‬ ‫ﺑﺮﺧﯽ‬ ‫ﺗﻌﯿﯿﻦ‬ ،‫ﺑﻌﺪ‬ ‫ﻣﺮﺣﻠﻪ‬‫ﻣـﺪت‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﮐﺸﺸﯽ‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻣﺎﻧﻨﺪ‬ ‫ﺑﺘﻦ‬ ‫اﯾﻦ‬ ‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺑﺮرﺳﯽ‬ ‫و‬-‫اﺳﺖ‬ ‫آن‬ ‫ﮐﺮﻧﺶ‬. ‫آزﻣﺎﯾﺸﮕﺎﻫﯽ‬ ‫اﻃﻼﻋﺎت‬ ‫ﻣﺼﺮﻓﯽ‬ ‫ﻣﺼﺎﻟﺢ‬ ‫ـﻪ‬‫ـ‬‫ﻧﻤﻮﻧ‬ ‫ـﮥ‬‫ـ‬‫ﻫﻤ‬ ‫ﺳـﺎﺧﺖ‬ ‫در‬‫ـﻮع‬‫ـ‬‫ﻧ‬ ‫ـﯿﻤﺎن‬‫ـ‬‫ﺳ‬ ،‫ﻫـﺎ‬I‫ـﯽ‬‫ـ‬‫ﺳﯿﻠﯿﺴ‬ ‫دوده‬ ، ،‫ازﻧـﺎ‬ ‫در‬ ‫واﻗـﻊ‬ ‫اﯾـﺮان‬ ‫ﻓﺮوآﻟﯿـﺎژ‬ ‫ﺻـﻨﺎﯾﻊ‬ ‫ﺷﺮﮐﺖ‬ ‫در‬ ‫ﺗﻮﻟﯿﺪﺷﺪه‬ ‫اﺳﺘﺨﺮاج‬ ‫اﺳﮑﻮرﯾﺎي‬ ‫و‬ ‫اﯾﺮاﻧﯽ‬ ‫داﻧﻪ‬‫ﻗـﺮوه‬ ‫از‬ ‫ﺷﺪه‬ 12‫ﻣﯿﻠﯽ‬‫درﺷﺖ‬ ‫ﻋﻨﻮان‬ ‫ﺑﻪ‬ ‫ﻣﺘﺮ‬‫رﯾﺰداﻧـﻪ‬ ،‫داﻧﻪ‬ ‫ـﯽ‬‫ـ‬‫اﻓﺰودﻧ‬ ‫ـﯿﻦ‬‫ـ‬‫ﻫﻤﭽﻨ‬ ‫و‬ ‫ـﺎك‬‫ـ‬‫ﻣﺘﻮﺳ‬ ‫ـﺮﮐﺖ‬‫ـ‬‫ﺷ‬ ‫ـﺪي‬‫ـ‬‫ﺗﻮﻟﯿ‬ ‫ـﻮﻟﯽ‬‫ـ‬‫ﻣﻌﻤ‬ ‫ﻣﺤ‬ ،‫ﻧﻔﺘﺎﻟﯿﻦ‬ ‫ﭘﺎﯾﻪ‬ ‫ﺑﺮ‬ ‫ﮐﻨﻨﺪه‬‫ب‬ ‫ﺷـﺮﮐﺖ‬ ‫ﺼـﻮل‬.‫آ‬.‫اس‬. ‫ﺷﺪ‬ ‫اﺳﺘﻔﺎده‬ ‫اﯾﺮاﻧﯿﺎن‬ ‫اف‬.‫ﻧﻤﻮﻧﻪ‬ ‫ﻫﻤﮥ‬ ‫در‬‫ﺧﺸـﮏ‬ ‫رﯾﺰداﻧﻪ‬ ‫از‬ ‫ﻫﺎ‬ ‫اﺳـﺖ‬ ‫ﺷـﺪه‬ ‫اﺳـﺘﻔﺎده‬ ‫ﺧﺸـﮏ‬ ‫ﺳـﺒﮏ‬ ‫داﻧﻪ‬. ‫ردﺷـﺪه‬ ‫درﺻـﺪ‬(‫ﺳـﺒﮏ‬‫داﻧـﻪ‬‫و‬ ‫ﻟﯿﮑـﺎ‬ ‫ﻫـﺎي‬ ‫ـﺘﺎﻧﺪارد‬‫ـ‬‫اﺳ‬ ‫ـﺪوده‬‫ـ‬‫ﻣﺤ‬ ‫در‬ ‫ـﮑﻮرﯾﺎ‬‫ـ‬‫اﺳ‬ASTM C330]18[‫ـﺮار‬‫ـ‬‫ﻗ‬ ‫ﻓﻮق‬ ‫و‬ ‫ﺳﯿﻤﺎن‬‫روان‬‫اﺳﺘﻔﺎده‬ ‫ﮐﻨﻨﺪه‬‫ﻧ‬ ‫ﺷﺪه‬‫ﺗﺮﺗﯿـﺐ‬ ‫ﺑـﻪ‬ ‫ﯿـﺰ‬ ASTM C]19[‫و‬ASTM C494]20[‫ـﻮده‬‫ـ‬‫ﺑ‬ ‫اﻧﺒﻮﻫﯽ‬ ‫ﺧﺸﮏ‬ ‫ﻓﻀﺎﯾﯽ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬(3Kg/m)‫ﺑﺮاي‬ ‫ﺗﺮﺗﯿـﺐ‬ ‫ﺑـﻪ‬ ‫اﺳـﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬430‫و‬702‫ﻣﺨﺼـﻮص‬ ‫وزن‬ ‫و‬ ‫ﻣﯿﻠـﻪ‬ ‫ﺑﺎ‬ ‫ﻣﺘﺮاﮐﻢ‬ ‫ﺧﺸﮏ‬ ‫ﻓﻀﺎﯾﯽ‬(3Kg/m)‫وزن‬‫ﻫـﺎ‬507‫و‬783 ‫اﻧﺒﻮﻫﯽ‬ ‫ﺧﺸﮏ‬ ‫ﻓﻀﺎﯾﯽ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﻣﯿﺰان‬ ‫ﺑﯿﺸﺘﺮﯾﻦ‬ ‫اﺳـﺘﺎﻧﺪارد‬ ‫ﻃﺒـﻖ‬ ‫ﺳـﺒﮏ‬ ‫ﻫﺎي‬ASTM C330، ‫اﺳﺖ‬ ‫ﺷﺪه‬ ‫ﻗﯿﺪ‬.‫آب‬ ‫ﺟﺬب‬24‫داﻧﻪ‬ ‫ﺳﺎﻋﺘﻪ‬‫ﻫـﺎي‬ ‫ﺗﺮﺗﯿﺐ‬ ‫ﺑﻪ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬8‫و‬5‫اﺳﺖ‬ ‫ﻣﯽ‬ ‫درﺻﺪ‬. ‫ﻣﺨﻠﻮط‬ ‫اﻧﺘﺨﺎب‬ ‫اﺻﻮل‬‫ﻧﺴﺒﺖ‬ ‫و‬ ‫ﻫﺎ‬‫آن‬ ‫ﻫﺎي‬‫ﻫﺎ‬ ‫ﺑﺮاي‬ ‫ﮔﻮﻧﺎﮔﻮن‬‫ﺳﺒﮏ‬ ‫ﺣﺠﻢ‬ ‫ﻣﻘﺎﯾﺴﻪ‬‫داﻧﻪ‬‫ﺑ‬ ‫ﻫﺎ‬‫ﺎ‬ ‫ـﺪ‬‫ـ‬‫ﺷ‬ ‫ـﻪ‬‫ـ‬‫ﺗﻬﯿ‬ ‫ـﺘﻦ‬‫ـ‬‫ﺑ‬ ‫ـﯽ‬‫ـ‬‫ﻓﯿﺰﯾﮑ‬ ‫ـﺎت‬‫ـ‬‫ﻣﺸﺨﺼ‬.‫ـﺮح‬‫ـ‬‫ﻃ‬ ‫ـﻦ‬‫ـ‬‫اﯾ‬ ‫در‬‫ـﺎ‬‫ـ‬‫ﻫ‬ ‫ﻣﻘﺪار‬ ‫ﺑﻪ‬ ‫ﻫﺎ‬10‫ﻃﺒﯿﻌﯽ‬ ‫ﻣﺎﺳﻪ‬ ‫ﺑﺎ‬ ‫ﺣﺠﻤﺸﺎن‬ ‫درﺻﺪ‬ ‫ﻣﺪرس‬ ‫ﻋﻤﺮان‬ ‫ﭘﮋوﻫﺸﯽ‬ 81 ‫ﺗﻮدﭼﯿﻨﯽ‬ ‫ﻣﻨﺤﻨﯽ‬]14[ ‫اﺻﻼح‬ ‫ﻣﻨﺤﻨﯽ‬‫ﻫﻮﮔﻨﺴﺘﺎد‬ ‫ﺷﺪه‬]13[ ‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺗﺤﻠﯿﻠﯽ‬ ‫ﺗﺨﻤﯿﻦ‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬ ‫ﺗـﻨﺶ‬ ‫ﻣﻨﺤﻨـﯽ‬ ‫ﺗﺨﻤـﯿﻦ‬ ‫ﺑﺮاي‬ ‫رواﺑﻄﯽ‬-‫ﮐـﺮﻧﺶ‬ ‫اﺳﺖ‬ ‫ﮐﺮده‬ ‫اراﺋﻪ‬ ‫ﭘﺎﯾﯿﻦ‬ ‫ﻫﺎي‬.‫ﺗﺨﻤﯿﻦ‬‫ﻫـﺎﯾﯽ‬ ‫ﺳـﻦ‬ ‫و‬ ‫ﻣﻘﺎوﻣـﺖ‬ ،‫ﺳﯿﻤﺎن‬ ‫ﺑﻪ‬ ‫آب‬ ‫از‬ ‫ﺷﺪه‬ ،‫ﻣﻮﺟـﻮد‬ ‫رواﺑـﻂ‬ ‫دﯾﮕـﺮ‬ ‫ﻃﺮﯾﻖ‬ ‫از‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﻪ‬ ‫ﻧﺴﺒﺖ‬ ‫اﺳﺖ‬ ‫زده‬ ‫اﺳـﺖ‬ ‫ﮐـﺮده‬ ‫اراﺋﻪ‬ ‫ﺗﺮي‬.‫ﭼـﻮ‬ ‫و‬ ‫ﮐﺮﯾـﺮا‬]16[‫ﻧﯿـﺰ‬ ‫اﻧﺪ‬.‫ﺑﻠﭽﻤﻦ‬]17[‫را‬ ‫ﻣﺘﻔـﺎوﺗﯽ‬ ‫رواﺑﻂ‬ ‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﻧﺰوﻟﯽ‬ ‫و‬ ‫ﺻﻌﻮدي‬ ‫ﻫﺎي‬-‫اراﺋـﻪ‬ ‫ﮐﺮﻧﺶ‬ ‫دارد‬ ‫ﻫﺪف‬ ‫دو‬ ‫ﭘﮋوﻫﺶ‬ ‫اﯾﻦ‬.‫از‬ ‫اﺳﺘﻔﺎده‬ ‫اﻣﮑﺎن‬ ‫اﺛﺒﺎت‬ ‫اﺑﺘﺪا‬ ‫ﺳـﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﺗﻮﻟﯿﺪ‬ ‫در‬ ‫ﮐﺸﻮر‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫ﻟﯿﮑﺎي‬ ‫و‬ ‫اﺳﮑﻮرﯾﺎ‬‫داﻧـﻪ‬ ‫ﻓـﻮق‬ ‫و‬ ‫ﻣﯿﮑﺮوﺳـﯿﻠﯿﺲ‬ ‫اﻓﺰودن‬ ‫ﺑﺎ‬ ‫ﭘﺮﻣﻘﺎوﻣﺖ‬‫روان‬‫در‬ ‫و‬ ‫ﮐﻨﻨـﺪه‬ ‫ﮐﻮﺗﺎه‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫از‬ ‫ﺑﺮﺧﯽ‬ ‫ﺗﻌﯿﯿﻦ‬ ،‫ﺑﻌﺪ‬ ‫ﻣﺮﺣﻠﻪ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﮐﺸﺸﯽ‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻣﺎﻧﻨﺪ‬ ‫ﺑﺘﻦ‬ ‫اﯾﻦ‬ ‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺑﺮرﺳﯽ‬ ‫و‬ 2-‫آزﻣﺎﯾﺸﮕﺎﻫﯽ‬ ‫اﻃﻼﻋﺎت‬ 1-2-‫ﻣﺼﺮﻓﯽ‬ ‫ﻣﺼﺎﻟﺢ‬ ‫ـﻪ‬‫ـ‬‫ﻧﻤﻮﻧ‬ ‫ـﮥ‬‫ـ‬‫ﻫﻤ‬ ‫ﺳـﺎﺧﺖ‬ ‫در‬ ،‫ازﻧـﺎ‬ ‫در‬ ‫واﻗـﻊ‬ ‫اﯾـﺮان‬ ‫ﻓﺮوآﻟﯿـﺎژ‬ ‫ﺻـﻨﺎﯾﻊ‬ ‫ﺷﺮﮐﺖ‬ ‫در‬ ‫ﺗﻮﻟﯿﺪﺷﺪه‬ ‫درﺷﺖ‬ ‫ﻟﯿﮑﺎي‬‫اﺳﺘﺨﺮاج‬ ‫اﺳﮑﻮرﯾﺎي‬ ‫و‬ ‫اﯾﺮاﻧﯽ‬ ‫داﻧﻪ‬ ‫اﻧﺪازه‬ ‫ﺑﯿﺸﯿﻨﮥ‬ ‫ﺑﺎ‬5/12 ‫ـﯽ‬‫ـ‬‫اﻓﺰودﻧ‬ ‫ـﯿﻦ‬‫ـ‬‫ﻫﻤﭽﻨ‬ ‫و‬ ‫ـﺎك‬‫ـ‬‫ﻣﺘﻮﺳ‬ ‫ـﺮﮐﺖ‬‫ـ‬‫ﺷ‬ ‫ـﺪي‬‫ـ‬‫ﺗﻮﻟﯿ‬ ‫ـﻮﻟﯽ‬‫ـ‬‫ﻣﻌﻤ‬ ‫ﻓﻮق‬‫روان‬‫ﻣﺤ‬ ،‫ﻧﻔﺘﺎﻟﯿﻦ‬ ‫ﭘﺎﯾﻪ‬ ‫ﺑﺮ‬ ‫ﮐﻨﻨﺪه‬ ‫ﺷﺪ‬ ‫اﺳﺘﻔﺎده‬ ‫اﯾﺮاﻧﯿﺎن‬ ‫اف‬ ‫درﺷﺖ‬ ‫و‬ ‫ﻣﻌﻤﻮﻟﯽ‬‫اﺳـﺖ‬ ‫ﺷـﺪه‬ ‫اﺳـﺘﻔﺎده‬ ‫ﺧﺸـﮏ‬ ‫ﺳـﺒﮏ‬ ‫داﻧﻪ‬ ‫داﻧﻪ‬‫وزﻧـﯽ‬ ‫ﺑﻨﺪي‬)‫ردﺷـﺪه‬ ‫درﺻـﺪ‬ ‫ـﺘﺎﻧﺪارد‬‫ـ‬‫اﺳ‬ ‫ـﺪوده‬‫ـ‬‫ﻣﺤ‬ ‫در‬ ‫ـﮑﻮرﯾﺎ‬‫ـ‬‫اﺳ‬ ‫داﺷﺖ‬.‫ﻓﻮق‬ ‫و‬ ‫ﺳﯿﻤﺎن‬ ‫ـﺮ‬‫ـ‬‫ﺑ‬ ‫ـﻖ‬‫ـ‬‫ﻣﻨﻄﺒ‬ASTM C150 ‫اﺳﺖ‬.‫اﻧﺒﻮﻫﯽ‬ ‫ﺧﺸﮏ‬ ‫ﻓﻀﺎﯾﯽ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﺗﺮﺗﯿـﺐ‬ ‫ﺑـﻪ‬ ‫اﺳـﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬ ‫ﻣﯿﻠـﻪ‬ ‫ﺑﺎ‬ ‫ﻣﺘﺮاﮐﻢ‬ ‫ﺧﺸﮏ‬ ‫ﻓﻀﺎﯾﯽ‬ ‫اﺳﺖ‬.‫اﻧﺒﻮﻫﯽ‬ ‫ﺧﺸﮏ‬ ‫ﻓﻀﺎﯾﯽ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﻣﯿﺰان‬ ‫ﺑﯿﺸﺘﺮﯾﻦ‬ ‫درﺷﺖ‬ ‫ﺑﺮاي‬‫داﻧﻪ‬‫اﺳـﺘﺎﻧﺪارد‬ ‫ﻃﺒـﻖ‬ ‫ﺳـﺒﮏ‬ ‫ﻫﺎي‬ (3Kg/m)880‫اﺳﺖ‬ ‫ﺷﺪه‬ ‫ﻗﯿﺪ‬ ‫ﺗﺮﺗﯿﺐ‬ ‫ﺑﻪ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬ 2-2-‫ﻣﺨﻠﻮط‬ ‫اﻧﺘﺨﺎب‬ ‫اﺻﻮل‬ ‫ﻣﺨﻠﻮط‬ ‫ﺷﺶ‬‫ﺑﺮاي‬ ‫ﮔﻮﻧﺎﮔﻮن‬ ‫ـﺪ‬‫ـ‬‫ﺷ‬ ‫ـﻪ‬‫ـ‬‫ﺗﻬﯿ‬ ‫ـﺘﻦ‬‫ـ‬‫ﺑ‬ ‫ـﯽ‬‫ـ‬‫ﻓﯿﺰﯾﮑ‬ ‫ـﺎت‬‫ـ‬‫ﻣﺸﺨﺼ‬ ‫ﺳﺒﮏ‬‫داﻧﻪ‬‫ﻣﻘﺪار‬ ‫ﺑﻪ‬ ‫ﻫﺎ‬ ‫ﻋﻠﻤﯽ‬ ‫ﻣﺠﻠﻪ‬-‫ﻣﺪرس‬ ‫ﻋﻤﺮان‬ ‫ﭘﮋوﻫﺸﯽ‬ ‫ﺗﻮدﭼﯿﻨﯽ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫اﺻﻼح‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺷﮑﻞ‬)1(‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺗﺤﻠﯿﻠﯽ‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﭘﻮﭘﻮوﯾﭻ‬]15[‫ﺗـﻨﺶ‬ ‫ﻣﻨﺤﻨـﯽ‬ ‫ﺗﺨﻤـﯿﻦ‬ ‫ﺑﺮاي‬ ‫رواﺑﻄﯽ‬ ‫ﺑﺘﻦ‬‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﺎ‬ ‫ﻫﺎي‬‫اﺳﺖ‬ ‫ﮐﺮده‬ ‫اراﺋﻪ‬ ‫ﭘﺎﯾﯿﻦ‬ ‫ﻫﺎي‬ ‫داده‬ ‫داﻣﻨﻪ‬ ‫در‬ ‫وي‬ ‫ﮐﻪ‬‫ﺳـﻦ‬ ‫و‬ ‫ﻣﻘﺎوﻣـﺖ‬ ،‫ﺳﯿﻤﺎن‬ ‫ﺑﻪ‬ ‫آب‬ ‫از‬ ‫ﺷﺪه‬ ،‫ﻣﻮﺟـﻮد‬ ‫رواﺑـﻂ‬ ‫دﯾﮕـﺮ‬ ‫ﻃﺮﯾﻖ‬ ‫از‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﻪ‬ ‫ﻧﺴﺒﺖ‬ ‫اﺳﺖ‬ ‫زده‬ ‫ﻣﻨﻄﻘﯽ‬ ‫ﻧﺘﺎﯾﺞ‬‫اﺳـﺖ‬ ‫ﮐـﺮده‬ ‫اراﺋﻪ‬ ‫ﺗﺮي‬ ‫ارا‬ ‫دﯾﮕﺮي‬ ‫راﺑﻄﻪ‬‫ﮐﺮده‬ ‫ﺋﻪ‬‫اﻧﺪ‬ ‫ﺷﺎﺧﻪ‬ ‫ﺑﺮاي‬‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﻧﺰوﻟﯽ‬ ‫و‬ ‫ﺻﻌﻮدي‬ ‫ﻫﺎي‬ ‫اﺳﺖ‬ ‫ﮐﺮده‬. ‫دارد‬ ‫ﻫﺪف‬ ‫دو‬ ‫ﭘﮋوﻫﺶ‬ ‫اﯾﻦ‬ ‫ﺳـﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﺗﻮﻟﯿﺪ‬ ‫در‬ ‫ﮐﺸﻮر‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫ﻟﯿﮑﺎي‬ ‫و‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﻓـﻮق‬ ‫و‬ ‫ﻣﯿﮑﺮوﺳـﯿﻠﯿﺲ‬ ‫اﻓﺰودن‬ ‫ﺑﺎ‬ ‫ﭘﺮﻣﻘﺎوﻣﺖ‬
  • 4. ‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫و‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﺮرﺳﯽ‬-‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫داﻧﻪ‬‫ﭼﺎﻟﻪ‬ ‫ﻋﻠﯿﺮﺿﺎ‬ ‫و‬ ‫ﺧﺎﻧﺰادي‬ ‫ﻣﺼﻄﻔﯽ‬‫ﮐﺎﯾﯽ‬ 82 ‫ﺷﺪ‬ ‫ﺟﺎﯾﮕﺰﯾﻦ‬.‫ﺣﺮوف‬L‫و‬S‫اﺧـﺘﻼط‬ ‫ﻃـﺮح‬ ‫ﻫﺮ‬ ‫ﻋﻨﻮان‬ ‫در‬ ‫اﺳـﺖ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﺑﺘﻦ‬ ‫ﺑﯿﺎﻧﮕﺮ‬ ‫ﺗﺮﺗﯿﺐ‬ ‫ﺑﻪ‬.‫ﻫﻤـﮥ‬ ‫ﻣﺨﻠﻮط‬‫ﺑﺎ‬ ‫ﺑﺘﻦ‬ ‫ﻫﺎي‬500‫ﺑـﺮ‬ ‫ﮐﯿﻠـﻮﮔﺮم‬‫ﻣـﻮاد‬ ‫ﻣﮑﻌـﺐ‬ ‫ﻣﺘـﺮ‬ ‫ﺳﯿﻤﺎﻧﯽ‬ ‫ﻣﻮاد‬ ‫ﺑﻪ‬ ‫ﺳﯿﻤﺎن‬ ‫وزﻧﯽ‬ ‫ﻧﺴﺒﺖ‬ ‫و‬ ‫ﺳﯿﻤﺎﻧﯽ‬3/0‫ﻃـﺮح‬ ‫ﺷﺪ‬.‫ﻃﺮح‬ ‫اﯾﻦ‬ ‫در‬‫ﻫﺎ‬450‫ﻧﻮع‬ ‫ﭘﺮﺗﻠﻨﺪ‬ ‫ﺳﯿﻤﺎن‬ ‫ﮐﯿﻠﻮﮔﺮم‬I‫ﺑﺎ‬ 50‫ﺷﺪ‬ ‫اﺳﺘﻔﺎده‬ ‫ﺳﯿﻠﯿﺴﯽ‬ ‫دوده‬ ‫ﮐﯿﻠﻮﮔﺮم‬.‫ﻣﺨﻠﻮط‬ ‫ﻫﻤﮥ‬ ‫از‬‫ﻫﺎ‬ ‫اﺳـﻼﻣﭗ‬ ‫اﻓﺖ‬ ‫ﻣﯿﺰان‬ ‫ﮐﻪ‬ ‫ﺷﺪ‬ ‫ﮔﺮﻓﺘﻪ‬ ‫اﺳﻼﻣﭗ‬ ‫اﻓﺖ‬ ‫آزﻣﺎﯾﺶ‬ ‫اﺧﺘﻼط‬ ‫ﻫﻤﮥ‬ ‫در‬‫ﻫﺎ‬10-8‫ﺳـﺎﻧﺘﯽ‬‫اﺳـﺖ‬ ‫ﺑـﻮده‬ ‫ﻣﺘـﺮ‬.‫ﺑـﺮ‬‫اي‬ ‫ﻓﻮق‬ ،‫ﻣﻮردﻧﻈﺮ‬ ‫ﮐﺎراﯾﯽ‬ ‫ﺑﻪ‬ ‫دﺳﺘﯿﺎﺑﯽ‬‫روان‬‫ﮐﻨﻨﺪه‬‫ﻣﯿـﺰان‬ ‫ﺑـﻪ‬ ‫اي‬ ‫ﺑـﺘﻦ‬ ‫ﺑـﻪ‬ ‫ﺳـﯿﻤﺎن‬ ‫وزن‬ ‫درﺻﺪ‬ ‫ﯾﮏ‬‫ﺷـﺪ‬ ‫اﺿـﺎﻓﻪ‬ ‫ﻫـﺎ‬.‫ﻫـﺮ‬ ‫از‬ ‫ﻧﻤﻮﻧـﻪ‬ ،‫اﺧﺘﻼط‬‫ﻣﮑﻌـﺐ‬ ‫ﻫـﺎي‬150‫ﻣﯿﻠـﯽ‬‫ﺳـﯿﻠﻨﺪر‬ ،‫ﻣﺘـﺮي‬ ‫ﻃـﻮل‬ ‫ﺑﺎ‬ ‫ﺳﯿﻠﻨﺪر‬ ‫و‬ ‫اﺳﺘﺎﻧﺪارد‬200‫ﻗﻄـﺮ‬ ‫و‬100‫ﻣﯿﻠـﯽ‬‫ﻣﺘـﺮ‬ ‫ﺳـﻦ‬ ‫در‬ ‫اﻻﺳﺘﯿﺴـﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺗﻌﯿﯿﻦ‬ ‫ﺑﺮاي‬ 28‫ﺷ‬ ‫ﺗﻬﯿﻪ‬ ‫روز‬‫ﺪ‬.‫ﻧﻤﻮﻧـﻪ‬ ‫ﻫﻤـﮥ‬‫ﻣﯿـﺰ‬ ‫روي‬ ‫ﻻﯾـﻪ‬ ‫دو‬ ‫در‬ ‫ﻫـﺎ‬ ‫ﺷﺪ‬ ‫ﻣﺘﺮاﮐﻢ‬ ‫وﯾﺒﺮه‬.‫آن‬ ‫ﺳﻄﺢ‬‫ﺗـﺮاز‬ ‫ﺷـﺪن‬ ‫ﻣﺘﺮاﮐﻢ‬ ‫از‬ ‫ﭘﺲ‬ ‫ﻫﺎ‬ ‫ﻗﺎﻟـﺐ‬ ‫در‬ ‫روز‬ ‫ﯾـﮏ‬ ‫ﻣﺪت‬ ‫ﺑﻪ‬ ‫و‬ ‫ﺷﺪ‬ ‫ﭘﺮداﺧﺖ‬ ‫ﻣﺎﻟﻪ‬ ‫ﺑﺎ‬ ،‫ﺷﺪه‬ ‫ﻧﮕﻪ‬‫ﻗﺎﻟﺐ‬ ‫ﺳﭙﺲ‬ ‫ﺷﺪ؛‬ ‫داري‬‫ﻧﻤﻮﻧﻪ‬ ‫و‬ ‫ﺷﺪ‬ ‫ﺑﺎز‬ ‫ﻫﺎ‬‫زﻣـﺎن‬ ‫ﺗـﺎ‬ ‫ﻫﺎ‬ ‫دﻣـﺎي‬ ‫ﺑـﺎ‬ ‫آب‬ ‫ﺣﻮﺿـﭽﻪ‬ ‫در‬ ‫آزﻣـﺎﯾﺶ‬ ‫اﻧﺠﺎم‬2±23‫درﺟـﻪ‬ ‫ﺳﺎﻧﺘﯽ‬‫ﻋﻤﻞ‬ ‫ﮔﺮاد‬‫ﺷﺪ‬ ‫آوري‬. ‫ﺟﺪول‬)1(‫ﻧﺴﺒﺖ‬ ‫و‬ ‫ﻣﻘﺎدﯾﺮ‬‫ﻣﺨﻠﻮط‬ ‫اﺟﺰاء‬ ‫ﻫﺎي‬‫آزﻣﺎﯾﺶ‬ ‫ﻫﺎي‬(3Kg/m) ‫ﻧﺎم‬ ‫اﺧﺘﻼط‬ ‫ﺳﯿﻤﺎن‬‫ﻣﯿﮑﺮوﺳﯿﻠﯿﺲ‬‫درﺷﺖ‬‫داﻧﻪ‬‫رﯾﺰداﻧﻪ‬ ‫آب‬ ‫آزاد‬ ‫وزن‬ ‫ﻣﺨﺼﻮص‬ ‫ﺗﺎزه‬ ‫ﺑﺘﻦ‬ L1450503157301501715 L2450502608601501790 L3450502059901501865 S1450505957281501998 S2450505018581502034 S3450504079881502070 ‫ﻧﺴﺒﺖ‬‫ﭘﯿﺸﻨﻬﺎدﺷـﺪه‬ ‫ﺷـﯿﻮه‬ ‫اﺳـﺎس‬ ‫ﺑﺮ‬ ‫اﺑﺘﺪا‬ ‫در‬ ‫ﺑﺘﻦ‬ ‫اﺧﺘﻼط‬ ‫ﻫﺎي‬ ‫در‬ACI 211.1]21[‫ﺷﺪ‬ ‫ﻣﻨﻈﻮر‬.‫ﺑﻪ‬ ‫رﺳﯿﺪن‬ ‫ﺗﺎ‬ ‫ﻣﻘﺎدﯾﺮ‬ ‫اﯾﻦ‬ ‫ﺳﭙﺲ‬ ‫ـﺪ‬‫ـ‬‫ﺷ‬ ‫ـﻪ‬‫ـ‬‫ﺑﻬﯿﻨ‬ ‫ـﺮ‬‫ـ‬‫ﻧﻈ‬ ‫ـﻮرد‬‫ـ‬‫ﻣ‬ ‫ـﺎري‬‫ـ‬‫ﻓﺸ‬ ‫ـﺖ‬‫ـ‬‫ﻣﻘﺎوﻣ‬.‫ـﺒﺖ‬‫ـ‬‫ﻧﺴ‬ ‫و‬ ‫ـﺎدﯾﺮ‬‫ـ‬‫ﻣﻘ‬ ‫ﻣﺨﻠﻮط‬‫ﺟﺪول‬ ‫در‬ ‫ﺑﺘﻦ‬ ‫ﻫﺎي‬)1(‫ﻣﯽ‬ ‫دﯾﺪه‬‫ﺷﻮد‬. 3-‫آن‬ ‫ﺗﻔﺴﯿﺮ‬ ‫و‬ ‫ﻧﺘﺎﯾﺞ‬‫ﻫﺎ‬ 3-1-‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻧﻤﻮﻧﻪ‬‫اﺳﺘﺎﻧﺪارد‬ ‫اﺳﺘﻮاﻧﻪ‬ ‫ﻫﺎي‬150×300‫ﻣﯿﻠـﯽ‬‫ﻣﮑﻌـﺐ‬ ‫و‬ ‫ﻣﺘـﺮ‬ 150‫ﻣﯿﻠﯽ‬‫ﺳـﻦ‬ ‫در‬ ‫ﻓﺸـﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫آزﻣﺎﯾﺶ‬ ‫و‬ ‫ﺳﺎﺧﺘﻪ‬ ‫ﻣﺘﺮي‬ 28‫ﺷـﺪ‬ ‫اﻧﺠﺎم‬ ‫آن‬ ‫روي‬ ‫روز‬.‫آزﻣـﺎﯾﺶ‬ ‫ﻧﺘـﺎﯾﺞ‬‫ﻣﻘﺎوﻣـﺖ‬ ‫ﻫـﺎي‬ ‫ﻧﻤﻮﻧﻪ‬ ‫روي‬ ‫ﻓﺸﺎري‬‫ﻫﺎي‬28‫ﻣﮑﻌﺐ‬ ‫روزه‬15‫ﺳـﺎﻧﺘﯽ‬‫و‬ ‫ﻣﺘـﺮي‬ ‫ﻧﻤﻮ‬ ‫ﺧﺸﮏ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﻧﯿﺰ‬ ‫و‬ ‫اﺳﺘﺎﻧﺪارد‬ ‫اﺳﺘﻮاﻧﻪ‬‫ﻧـﻪ‬‫در‬ ‫ﻫـﺎ‬ ‫ﺟﺪول‬)2(‫اﺳﺖ‬ ‫ﺷﺪه‬ ‫اراﺋﻪ‬. ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﯿﺸﺘﺮﯾﻦ‬28‫ﺑـﺘﻦ‬ ‫روزه‬‫ﺣـﺎوي‬ ‫ﻫـﺎي‬ ‫ﻃﺮح‬ ،‫ﻟﯿﮑﺎ‬L3‫اﺳﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫در‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬‫اي‬MPa4/38‫و‬ ‫ﻣﮑﻌﺒﯽ‬ ‫ﻧﻤﻮﻧﻪ‬MPa85/40‫ﺑﻪ‬‫اﺳـﺖ‬ ‫آﻣـﺪه‬ ‫دﺳﺖ‬.‫اﯾـﻦ‬ ‫در‬ ‫ﺧﺸﮏ‬ ‫ﺑﺘﻦ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﺣﺎﻟﺖ‬kg/m31735‫ﺑـﻪ‬‫دﺳـﺖ‬ ‫ـﺖ‬‫ـ‬‫اﺳ‬ ‫ـﺪه‬‫ـ‬‫آﻣ‬.‫ـﺎري‬‫ـ‬‫ﻓﺸ‬ ‫ـﺖ‬‫ـ‬‫ﻣﻘﺎوﻣ‬ ‫ـﺘﺮﯾﻦ‬‫ـ‬‫ﺑﯿﺸ‬28‫ـﯿﻦ‬‫ـ‬‫ﺑ‬ ‫روزه‬ ‫ﺑ‬‫ﺘﻦ‬‫ﻣﺨﻠﻮط‬ ‫ﺑﻪ‬ ‫ﻣﺮﺑﻮط‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬S3‫ﮐـﻪ‬ ‫اﺳـﺖ‬ ‫ـﺮ‬‫ـ‬‫ﺑﺮاﺑ‬ ‫ـﯽ‬‫ـ‬‫ﻣﮑﻌﺒ‬ ‫ـﻪ‬‫ـ‬‫ﻧﻤﻮﻧ‬ ‫ـﺮاي‬‫ـ‬‫ﺑ‬MPa63/54‫ـﻪ‬‫ـ‬‫ﻧﻤﻮﻧ‬ ‫ـﺮاي‬‫ـ‬‫ﺑ‬ ‫و‬ ‫اﺳﺘﻮاﻧﻪ‬‫ﺑﺮاﺑﺮ‬ ‫اي‬MPa62/48‫اﺳـﺖ‬.‫ﺑـﺘﻦ‬ ‫ﻣﺨﺼـﻮص‬ ‫وزن‬ ‫ﺧﺸﮏ‬‫ﺣـﺪود‬ ‫ﻃـﺮح‬ ‫اﯾـﻦ‬ ‫ﺑـﻪ‬ ‫ﻣﺮﺑـﻮط‬ ‫ﺷـﺪه‬kg/m31940 ‫ﺑﻪ‬‫اﺳﺖ‬ ‫آﻣﺪه‬ ‫دﺳﺖ‬.‫ﻣﻘﺎوﻣﺖ‬ ‫ﻧﺘﺎﯾﺞ‬‫ﻓﺸـﺎري‬ ‫ﻫﺎي‬28‫روزه‬ ‫آزﻣﻮﻧﻪ‬ ‫وزن‬ ‫ﺗﺎﺑﻊ‬ ً‫ﻼ‬‫ﻋﻤ‬‫ﺑ‬ ‫و‬ ‫اﺳﺖ‬ ‫ﻫﺎ‬‫ﻣﻘﺎوﻣـﺖ‬ ،‫آن‬ ‫ﮐـﺎﻫﺶ‬ ‫ﺎ‬ ‫ﻣﯽ‬ ‫ﮐﺎﻫﺶ‬ ‫ﻧﯿﺰ‬‫ﯾﺎﺑﺪ‬.‫ﻧﻤﻮﻧـﻪ‬ ‫ﻓﺸـﺎري‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﻧﺴﺒﺖ‬‫ﻫـﺎي‬ ‫اﺳﺘﻮاﻧﻪ‬‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬ ‫ﻣﮑﻌﺐ‬ ‫ﺑﻪ‬ ‫اي‬‫ﺣـﺪود‬ ‫ﻟﯿﮑـﺎ‬ ‫ﺣـﺎوي‬ ‫ﻫـﺎي‬ 93/0‫ﻧﻤﻮﻧﻪ‬ ‫ﺑﺮاي‬ ‫و‬‫ﺣﺪود‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬87/0‫ﺛﺒﺖ‬ ‫اﺳـﺖ‬ ‫ﺷﺪه‬.‫ﻧﮑـﺎت‬ ‫رﻋﺎﯾـﺖ‬ ‫ﺑـﺎ‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﺑﯿﺸـﺘﺮ‬ ‫اﻓـﺰاﯾﺶ‬ ‫ﻣﺤﺪوده‬ ‫در‬ ‫ﺧﺸﮏ‬ ‫ﺑﺘﻦ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﺣﻔﻆ‬ ‫و‬ ‫اﻗﺘﺼﺎدي‬ ‫ﺑﺘﻦ‬‫ﺳـﺒﮏ‬ ‫ﻫﺎي‬‫ﻧﯿﺴـﺖ‬ ‫ﻣﻘـﺪور‬ ً‫ﻼ‬‫ﻋﻤـ‬.‫ﻣﻘﺎوﻣـﺖ‬ ‫اﻓـﺰاﯾﺶ‬ ‫ﺑﺘﻦ‬‫ﺗﺤﻘﯿﻘـﺎت‬ ‫ﺑـﻪ‬ ‫ﻧﺴﺒﺖ‬ ‫ﭘﮋوﻫﺶ‬ ‫اﯾﻦ‬ ‫در‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬ ‫داﻧﻪ‬ ‫ﻧﻮع‬ ‫ﺗﻔﺎوت‬ ‫دﻟﯿﻞ‬ ‫ﺑﻪ‬ ‫اﯾﺮان‬ ‫در‬ ‫ﮔﺬﺷﺘﻪ‬‫ﻟﯿﮑﺎﻫـﺎي‬ ‫ﺑـﺎ‬ ‫ﻫـﺎ‬ ‫اﺳﺘﻔﺎده‬‫اﺳﺖ‬ ‫ﺗﺤﻘﯿﻘﺎت‬ ‫آن‬ ‫در‬ ‫ﺷﺪه‬.
  • 5. ‫ﻋﻠﻤﯽ‬ ‫ﻣﺠﻠﻪ‬-‫ﻣﺪرس‬ ‫ﻋﻤﺮان‬ ‫ﭘﮋوﻫﺸﯽ‬‫ﺷﻤﺎره‬ ،‫دوازدﻫﻢ‬ ‫دوره‬4/‫زﻣﺴﺘﺎن‬1391 83 ‫ﺟﺪول‬)2(‫آزﻣﺎﯾﺶ‬ ‫ﻧﺘﺎﯾﺞ‬‫ﻧﻤﻮﻧﻪ‬ ‫روي‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻫﺎي‬‫ﻣﮑﻌﺐ‬ ‫ﻫﺎي‬ 15‫ﺳﺎﻧﺘﯽ‬‫اﺳﺘﺎﻧﺪارد‬ ‫اﺳﺘﻮاﻧﻪ‬ ‫و‬ ‫ﻣﺘﺮي‬ ‫ﻧﺎم‬ ‫ﻃﺮح‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻣﮑﻌﺐ‬ ‫ﻓﺸﺎري‬ (MPa) ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻓﺸﺎري‬ ‫اﺳﺘﻮاﻧﻪ‬(MPa) ‫وزن‬ ‫ﻣﺨﺼﻮص‬ ‫ﺧﺸﮏ‬ (3Kg/m) ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻧﺴﺒﺖ‬ ‫ﻧﻤﻮﻧﻪ‬‫اﺳﺘﻮاﻧﻪ‬ ‫ﻫﺎي‬ ‫ﻣﮑﻌﺐ‬ ‫ﺑﻪ‬ L120/3354/30158592/0 L229/3675/33166093/0 L385/4040/38173594/0 S135/4500/39186886/0 S246/5090/43190487/0 S363/5462/48194089/0 ‫داﻧﻪ‬ ،‫ﻟﯿﮑﺎ‬ ‫ﺷﺮﮐﺖ‬ ‫ﺗﻮﻟﯿﺪﮐﻨﻨﺪﮔﺎن‬ ‫اﻇﻬﺎر‬ ‫ﺑﻪ‬ ‫ﺑﻨﺎ‬‫ﺷﺪه‬ ‫اﺳﺘﻔﺎده‬ ‫ﻫﺎي‬ ‫دارﻧﺪ‬ ‫ﺑﻬﺘﺮي‬ ‫ﮐﯿﻔﯿﺖ‬ ‫ﭘﮋوﻫﺶ‬ ‫اﯾﻦ‬ ‫در‬. ‫ﺳﺒﮏ‬ ‫اﺷﻐﺎل‬ ‫ﺣﺠﻢ‬ ‫ﺗﺄﺛﯿﺮ‬‫داﻧﻪ‬‫ﺧـﻮﺑﯽ‬ ‫ﺑـﻪ‬ ‫ﻧﯿـﺰ‬ ‫ﺑﺘﻦ‬ ‫در‬ ‫ﻫﺎ‬ ‫ﻣﯽ‬ ‫دﯾﺪه‬‫ﺷﻮد‬.‫درﺷﺖ‬ ‫ﺑﺎﻓﺖ‬‫ﺳـﺒﮏ‬ ‫اﻓـﺰاﯾﺶ‬ ‫ﯾﻌﻨـﯽ‬ ‫ﺗﺮ‬‫داﻧـﻪ‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫داﺷﺘﻪ‬ ‫ﻧﺘﯿﺠﻪ‬ ‫دو‬ ،‫ﻣﻌﻤﻮﻟﯽ‬ ‫ﻣﺎﺳﻪ‬ ‫ﮐﺎﻫﺶ‬ ‫و‬ ‫درﺷﺖ‬ ‫ﻓﺸـﺎري‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﮐـﺎﻫﺶ‬ ‫و‬ ‫ﺑـﺘﻦ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬ ‫ﮐﺎﻫﺶ‬ ‫ﺳـﻨﮓ‬ ‫ﺑﺨـﺶ‬ ‫در‬ ‫ﺗﺨﻠﺨﻞ‬ ‫و‬ ‫ﭘﻮﮐﯽ‬ ‫زﯾﺮا‬ ‫اﺳﺖ؛‬‫ﺑﯿﺸـﺘﺮ‬ ‫داﻧـﻪ‬ ‫اﺳـﺖ‬ ‫ﺷﺪه‬ ‫اﯾﺠﺎد‬ ‫ﺑﯿﺸﺘﺮي‬ ‫ﺿﻌﻒ‬ ‫و‬ ‫ﺷﺪه‬.‫ﻣﻘـﺪار‬ ‫ﮐـﺎﻫﺶ‬ ‫ﺳﺒﮏ‬‫ﻣﺨﻠـﻮط‬ ‫ﻃـﺮح‬ ‫روش‬ ‫از‬ ‫اﺳـﺘﻔﺎده‬ ‫ﺑـﻪ‬ ‫ﺗﻮﺟـﻪ‬ ‫ﺑـﺎ‬ ‫داﻧﻪ‬ ‫درﺷـﺖ‬ ‫ﻣﻘﺪار‬ ‫ﺗﻌﯿﯿﻦ‬ ‫ﺑﺨﺶ‬ ‫در‬ ‫آﻣﺮﯾﮑﺎﯾﯽ‬‫اﻓـﺰاﯾﺶ‬ ‫و‬ ‫داﻧـﻪ‬ ‫ـﺒﮏ‬‫ـ‬‫ﺳ‬ ‫ـﻦ‬‫ـ‬‫ﺷ‬ ‫ـﺎﻫﺶ‬‫ـ‬‫ﮐ‬ ‫ـﻞ‬‫ـ‬‫دﻟﯿ‬ ‫ـﻪ‬‫ـ‬‫ﺑ‬ ‫ـﻮﻟﯽ‬‫ـ‬‫ﻣﻌﻤ‬ ‫ـﻪ‬‫ـ‬‫ﻣﺎﺳ‬ ‫ـﺪار‬‫ـ‬‫ﻣﻘ‬‫و‬ ‫ﺑﻪ‬‫ﭼﺸـﻢ‬ ‫اﻓـﺰاﯾﺶ‬ ‫ﺳﺒﺐ‬ ‫ﻣﻄﻠﻖ‬ ‫ﺣﺠﻢ‬ ‫ﻓﺮﻣﻮل‬ ‫ﮐﺎرﮔﯿﺮي‬‫ﮔﯿـﺮ‬ ‫ﻣﯽ‬ ‫ﺑﺘﻦ‬ ‫ﻣﺨﺼﻮص‬ ‫وزن‬‫ﺑـﺎﻻﺗﺮ‬ ‫ﻓﺸـﺎري‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫و‬ ‫ﺷـﻮد‬ ‫ﻣﯽ‬‫رود‬.‫ﻣﯽ‬ ‫را‬ ‫دﯾﮕﺮ‬ ‫دﻟﯿﻞ‬ ‫اﻣﺎ‬‫ﮐﯿﻔﯿـﺖ‬ ‫رﻓـﺘﻦ‬ ‫ﺑـﺎﻻ‬ ‫در‬ ‫ﺗـﻮان‬ ‫ﺳﺒﮏ‬‫داﻧﺴﺖ‬ ‫درﺷﺖ‬ ‫داﻧﻪ‬.‫آزﻣﺎﯾﺶ‬ ‫ﻧﺘﺎﯾﺞ‬ ‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬ ‫ﺑﺎ‬‫ﻫـﺎي‬ ‫ﻣﯽ‬ ‫ﻧﻈﺮ‬ ‫ﺑﻪ‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬‫ﺳﯿﻠﯿﺴـﯽ‬ ‫دوده‬ ‫ﻣﺼـﺮف‬ ‫رﺳـﺪ‬ ‫ﺑـﺘﻦ‬ ‫ﺑـﺮ‬ ‫ﺧـﻮﺑﯽ‬ ‫ﺗﺄﺛﯿﺮ‬‫ﻫـﺎ‬‫آزﻣـﺎﯾﺶ‬ ‫ي‬‫اﺳـﺖ‬ ‫داﺷـﺘﻪ‬ ‫ﺷـﺪه‬. ‫ﺗﺤﻠﯿﻞ‬‫ﻣﻨﻄﻘـﻪ‬ ‫ﺑﻬﺒـﻮد‬ ‫در‬ ‫ﺑﺎﯾـﺪ‬ ‫را‬ ‫ﻋﻠﺖ‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫ﻣﺪﻋﯽ‬ ‫ﮔﺮ‬ ‫ﺑﻪ‬ ‫ﺗﻤﺎس‬‫ﺟﺴـﺖ‬ ‫ﺳﯿﻠﯿﺴـﯽ‬ ‫دوده‬ ‫وﺳـﯿﻠﮥ‬‫ﮐـﺮد‬ ‫وﺟـﻮ‬.‫دوده‬ ‫ﻣـﯽ‬ ‫اﺟـﺎزه‬ ‫ﺳﯿﻠﯿﺴﯽ‬‫ﻧﺰدﯾﮑـﯽ‬ ‫در‬ ‫ﺑﺘﻮاﻧـﺪ‬ ‫ﻣـﺎده‬ ‫اﯾـﻦ‬ ‫دﻫـﺪ‬ ‫ﺳﺒﮏ‬‫ﻫﯿﺪروﮐﺴـﯿﺪ‬ ‫ﺑﻠﻮرﻫـﺎي‬ ‫از‬ ‫ﺗـﻮﺟﻬﯽ‬ ‫ﻗﺎﺑﻞ‬ ‫ﻣﻘﺎدﯾﺮ‬ ‫داﻧﻪ‬ ‫ﻣﺤﺼـﻮﻻت‬ ‫و‬ ‫رﺳـﺎﻧﺪ‬ ‫ﻣﺼﺮف‬ ‫ﺑﻪ‬ ‫و‬ ‫ﮐﺮده‬ ‫ﺟﺬب‬ ‫را‬ ‫ﮐﻠﺴﯿﻢ‬ ‫ﻧﻔ‬‫ﻣﻘﺎوم‬ ‫و‬ ‫ﻮذﻧﺎﭘﺬﯾﺮﺗﺮ‬‫ﺷﻮد‬ ‫ﺣﺎﺻﻞ‬ ‫ﺗﺮي‬.‫در‬ ‫رﻃﻮﺑﺖ‬ ‫وﺟﻮد‬ ‫ﺳﺒﮏ‬‫ﻋﻤـﻞ‬ ‫ﻣﺴﺌﻠﻪ‬ ‫و‬ ‫داﻧﻪ‬‫ﮐﻤـﮏ‬ ‫ﻧﯿـﺰ‬ ‫داﺧﻠـﯽ‬ ‫آوري‬‫ﮐﻨﻨـﺪه‬ ‫اﺳﺖ‬.‫ﺑﻪ‬ ‫ﻧﺘﺎﯾﺞ‬ ‫در‬ ‫ﺗﻮﺟﻪ‬ ‫ﻗﺎﺑﻞ‬ ‫ﻧﮑﺘﻪ‬‫دﺳﺖ‬‫ﻣﻘﺎوﻣـﺖ‬ ‫از‬ ‫آﻣﺪه‬ ‫ﻧﻤﻮﻧﻪ‬ ‫ﻓﺸﺎري‬‫اﺳﺘﻮاﻧﻪ‬ ‫و‬ ‫ﻣﮑﻌﺒﯽ‬ ‫ﻫﺎي‬‫ﻣﻘﺎوﻣـﺖ‬ ‫ﻧﺴـﺒﺖ‬ ،‫اي‬ ‫اﺳﺘﻮاﻧﻪ‬‫اﺳـﺖ‬ ‫ﻣﮑﻌﺒـﯽ‬ ‫ﺑﻪ‬ ‫اي‬.‫ﻧﻤﻮﻧـﻪ‬ ‫در‬ ‫ﻣﻘـﺪار‬ ‫اﯾـﻦ‬‫ﻫـﺎي‬ ‫ﻣﺤﺪ‬ ‫در‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬‫وده‬9/0‫اﺳـﺖ‬ ‫ﺑـﻮده‬ ‫ﺑﯿﺸـﺘﺮ‬ ‫ﺣﺘـﯽ‬ ‫و‬. ‫اﺳـﺘﻮاﻧﻪ‬ ‫از‬ ‫ﺑـﯿﺶ‬ ‫را‬ ‫ﻣﮑﻌﺒـﯽ‬ ‫ﺑـﺘﻦ‬ ‫ﻣﻘﺎوﻣﺖ‬ ،‫ﺟﺪاﺷﺪﮔﯽ‬‫اي‬ ‫ﻣﯽ‬ ‫ﮐﺎﻫﺶ‬‫ﺳـﺮﯾﻊ‬ ‫ﺧﺮدﺷﺪﮔﯽ‬ ‫و‬ ‫ﺷﮑﻞ‬ ‫ﺗﻐﯿﯿﺮ‬ ‫زﯾﺮا‬ ‫دﻫﺪ؛‬‫ﺗـﺮ‬ ‫ﺳﺒﺐ‬ ‫ﻓﺸﺎر‬ ‫دﺳﺘﮕﺎه‬ ‫زﯾﺮ‬ ‫در‬ ‫ﻣﮑﻌﺒﯽ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫در‬ ‫ﻗﺎﺋﻢ‬ ‫ﻻﯾﻪ‬ ‫ﯾﮏ‬ ‫ﻣﯽ‬ ‫ﻣﮑﻌﺒﯽ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫ﺑﯿﺸﺘﺮ‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﮐﺎﻫﺶ‬‫ﺷﻮد‬.‫ﮐﻪ‬ ‫ﺣﺎﻟﯽ‬ ‫در‬ ‫اﺳﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫در‬‫ﺿﻌﯿ‬ ‫ﻣﻨﻄﻘﻪ‬ ‫اﯾﻦ‬ ‫اي‬‫ﺗـﺄﺛﯿﺮ‬ ‫و‬ ‫ﺑﻮده‬ ‫اﻓﻘﯽ‬ ‫ﻒ‬ ‫دارد‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﮐـﺎﻫﺶ‬ ‫ﺑـﺮ‬ ‫ﮐﻤﺘﺮي‬.‫ﭘـﺮ‬ ‫ﻻﯾـﻪ‬ ‫ﯾـﮏ‬ ‫وﺟـﻮد‬ ‫ﺑﻪ‬ ‫ﻣﻘﺎوﻣﺖ‬‫دﺳﺖ‬‫ﭘﻮﺷﺶ‬ ‫ﻣﻮاد‬ ‫از‬ ‫آﻣﺪه‬‫ﮐـﻪ‬ ‫ﮐﻼﻫـﮏ‬ ‫دﻫﻨـﺪه‬ ‫ﺳـﺒﮏ‬ ‫ﺑـﺘﻦ‬ ‫ﺑـﻪ‬ ‫ﻧﺴﺒﺖ‬ ‫ﺑﯿﺸﺘﺮي‬ ‫ﻣﻘﺎوﻣﺖ‬‫ﺑﺎﻋـﺚ‬ ،‫دارد‬ ‫داﻧـﻪ‬ ‫اﺳﺘﻮاﻧﻪ‬ ‫آزﻣﻮﻧﻪ‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫اﻓﺰاﯾﺶ‬‫ﻣـﯽ‬ ‫اي‬‫ﺷـﻮد‬.‫اﺛـﺮ‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﺑﺮ‬ ‫اﻧﺘﻬﺎﯾﯽ‬ ‫ﺷﺮاﯾﻂ‬‫ﻣﻌﻤـﻮﻟﯽ‬ ‫ﺑـﺘﻦ‬ ‫از‬ ‫ﮐﻤﺘـﺮ‬ ‫داﻧـﻪ‬ ‫ا‬‫ﺳﺖ‬.‫ﭼﻨـﺪان‬ ‫ﻣﮑﻌﺒـﯽ‬ ‫ﻧﻤﻮﻧـﻪ‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫اﻓـﺰاﯾﺶ‬ ‫ﺑﻨﺎﺑﺮاﯾﻦ‬ ‫ﭼﺸﻢ‬‫ﻧﯿﺴﺖ‬ ‫ﮔﯿﺮ‬.‫ﺑـﺘﻦ‬ ‫در‬ ‫ﮐﻪ‬ ‫داﻧﯿﻢ‬ ‫ﻣﯽ‬‫ﻣﻘﺎوﻣـﺖ‬ ‫ﭘـﺮ‬ ‫ﻫـﺎي‬ ‫اﺳﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻧﺴﺒﺖ‬ ،‫ﻓﺸﺎري‬‫ﻣﮑﻌﺒﯽ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫ﺑﻪ‬ ‫اي‬ ‫ﻣﯽ‬ ‫ﻧﺰدﯾﮏ‬ ‫ﯾﮏ‬ ‫ﻋﺪد‬ ‫ﺑﻪ‬‫ﺷﻮد‬.‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬‫ﺳﺒﮏ‬ ‫ﻫﺎي‬‫اﯾـﻦ‬ ‫داﻧﻪ‬ ‫ﭘـﺲ‬ ‫اﺳـﺖ؛‬ ‫ﺑـﻮده‬ ‫ﮐـﻢ‬ ‫ﺳـﯿﻤﺎن‬ ‫ﺑـﻪ‬ ‫آب‬ ‫ﻧﺴـﺒﺖ‬ ،‫ﭘﮋوﻫﺶ‬ ‫ﻧﺰدﯾ‬ ‫ﺧﺎﻃﺮ‬ ‫ﺑﻪ‬ ‫آن‬ ‫ﮔﺴﯿﺨﺘﮕﯽ‬‫ﺳﻨﮓ‬ ‫ارﺗﺠﺎﻋﯽ‬ ‫ﻣﺪول‬ ‫ﮑﯽ‬‫داﻧﻪ‬ ‫ﺳـﻨﮓ‬ ‫و‬ ‫اﺳﺖ‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﭘﺮ‬ ‫ﺑﺘﻦ‬ ‫ﺷﺒﯿﻪ‬ ،‫ﺳﯿﻤﺎن‬ ‫ﺧﻤﯿﺮ‬ ‫و‬‫داﻧـﻪ‬ ‫ـﯽ‬‫ـ‬‫ﻣ‬ ‫ـﺮد‬‫ـ‬‫ﺧ‬ ‫ـﺮ‬‫ـ‬‫زودﺗ‬ ‫آن‬‫ـﯿﻦ‬‫ـ‬‫ﺑ‬ ‫از‬ ‫ـﺮك‬‫ـ‬‫ﺗ‬ ‫ـﺎرﺗﯽ‬‫ـ‬‫ﻋﺒ‬ ‫ـﻪ‬‫ـ‬‫ﺑ‬ ‫و‬ ‫ـﻮد‬‫ـ‬‫ﺷ‬ ‫ﺳﻨﮓ‬‫داﻧﻪ‬‫ﻣﯽ‬ ‫ﻋﺒﻮر‬ ‫ﻫﺎ‬‫ﺑـﻪ‬ ‫ﻧﺴﺒﺖ‬ ‫اﯾﻦ‬ ‫ﻧﺰدﯾﮑﯽ‬ ‫ﺑﻨﺎﺑﺮاﯾﻦ‬ ‫ﮐﻨﺪ؛‬ ‫اﺳﺖ‬ ‫ﻣﻨﻄﻘﯽ‬ ‫ﯾﮏ‬. ‫رﯾﻠﻢ‬‫اﺳﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫در‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫ﻣﻌﺘﻘﺪ‬ ،‫ﺧﻮاص‬ ‫اﺛﺮ‬ ‫اي‬ ‫ﺳﻨﮓ‬‫ﻓ‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﺮ‬ ‫درﺷﺖ‬ ‫داﻧﻪ‬‫ﻣﯽ‬ ‫ﮐﺎﻫﺶ‬ ‫ﺸﺎري‬‫ﯾﺎﺑﺪ‬]22[‫؛‬ ‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫در‬ ‫ﭘﺲ‬‫ﺳﻨﮓ‬ ،‫داﻧﻪ‬‫در‬ ‫ﮐـﺎﻫﺶ‬ ‫اﺛـﺮ‬ ‫درﺷـﺖ‬ ‫داﻧﻪ‬
  • 6. ‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫و‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﺮرﺳﯽ‬-‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫داﻧﻪ‬‫ﭼﺎﻟﻪ‬ ‫ﻋﻠﯿﺮﺿﺎ‬ ‫و‬ ‫ﺧﺎﻧﺰادي‬ ‫ﻣﺼﻄﻔﯽ‬‫ﮐﺎﯾﯽ‬ 84 ‫دارد‬ ‫ﻣﻘﺎوﻣﺖ‬.‫اﺳـﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫در‬ ‫ﺗﺄﺛﯿﺮ‬ ‫اﯾﻦ‬‫از‬ ‫ﻧـﺎﭼﯿﺰﺗﺮ‬ ‫اي‬ ‫ﻣﯽ‬ ‫ﻣﮑﻌﺒﯽ‬ ‫ﻧﻤﻮﻧﻪ‬‫ﻣﻘﺎوﻣﺖ‬ ‫و‬ ‫ﺷﻮد‬‫ﻧﻤﻮﻧـﻪ‬ ‫ﻧـﻮع‬ ‫دو‬ ‫اﯾﻦ‬ ‫ﻫﺎي‬ ‫ﻣﯽ‬ ‫ﻧﺰدﯾﮑﺘﺮ‬ ‫ﯾﮑﺪﯾﮕﺮ‬ ‫ﺑﻪ‬‫ﺷﻮد‬.‫در‬ ‫ﻧﺴﺒﺖ‬ ‫اﯾﻦ‬ ‫دﯾﮕﺮ‬ ‫ﺳﻮي‬ ‫از‬ ‫ﻧﻤﻮﻧﻪ‬‫ﮐﻤﺘ‬ ‫ﭼﻪ‬ ‫اﮔﺮ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬‫اﻣـﺎ‬ ‫ﺑـﻮده‬ ‫ﻟﯿﮑﺎ‬ ‫از‬ ‫ﺮ‬ ‫اﺳﺖ‬ ‫ﻣﻌﻤﻮﻟﯽ‬ ‫ﺑﺘﻦ‬ ‫از‬ ‫ﺑﯿﺸﺘﺮ‬ ‫ﻫﻢ‬ ‫ﺑﺎز‬.‫ﻧﻈـﺮ‬ ‫ﺑـﻪ‬ ‫ﻣﻮرد‬ ‫اﯾﻦ‬ ‫در‬ ‫ﻣﯽ‬‫ﻣﻌﻤـﻮﻟﯽ‬ ‫ﺑﺘﻦ‬ ‫ﺑﻪ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﺑﺘﻦ‬ ‫ﺧﺼﻮﺻﯿﺎت‬ ‫رﺳﺪ‬ ‫ﻧﺰدﯾﮏ‬‫اﺳﺖ‬ ‫ﺗﺮ‬. 3-2-‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﺳـﻦ‬ ‫در‬ ‫اﺳـﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴـﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫آزﻣﺎﯾﺶ‬28‫روي‬ ‫روز‬ ‫ـﻪ‬‫ـ‬‫ﻧﻤﻮﻧ‬‫ـﺘﺎﻧﺪارد‬‫ـ‬‫اﺳ‬ ‫ـﺎي‬‫ـ‬‫ﻫ‬150×300‫ـﯽ‬‫ـ‬‫ﻣﯿﻠ‬‫ـﺎس‬‫ـ‬‫اﺳ‬ ‫ـﺮ‬‫ـ‬‫ﺑ‬ ‫و‬ ‫ـﺮ‬‫ـ‬‫ﻣﺘ‬ ‫ﻣﺸﺨﺼﺎت‬ASTM‫ﺷﺪ‬ ‫اﻧﺠﺎم‬.‫ﺟﺪول‬ ‫در‬)3(‫آزﻣـﺎﯾﺶ‬ ‫ﻧﺘﺎﯾﺞ‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬28،‫ﻣﺨﺼـﻮص‬ ‫وزن‬ ‫ﻫﻤﺮاه‬ ‫روزه‬ ‫ﻣﯽ‬ ‫ﻣﺸﺎﻫﺪه‬ ‫ﺑﺘﻦ‬ ‫ﺑﺮﺷﯽ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﭘﻮاﺳﻮن‬ ‫ﺿﺮﯾﺐ‬‫ﮔﺮدد‬. ‫ﺟﺪول‬)4(‫راﯾﺞ‬ ‫از‬ ‫ﺑﺮﺧﯽ‬‫ﭘـﯿﺶ‬ ‫ﺑـﺮاي‬ ‫رواﺑﻂ‬ ‫ﺗﺮﯾﻦ‬‫ﺑﯿﻨـﯽ‬ ‫ﻣﯽ‬ ‫ﻧﺸﺎن‬ ‫را‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬‫دﻫﺪ‬.‫ﺟـ‬ ‫در‬‫ﺪول‬)5( ‫ﺑﻪ‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﻧﺘﺎﯾﺞ‬‫دﺳﺖ‬‫ﺑـﺎ‬ ‫آزﻣﺎﯾﺸﻬﺎ‬ ‫از‬ ‫آﻣﺪه‬ ‫ﺗﺨﻤﯿﻦ‬‫زده‬ ‫ﻫﺎي‬‫اﺳﺖ‬ ‫ﺷﺪه‬ ‫ﻣﻘﺎﯾﺴﻪ‬ ‫راﯾﺞ‬ ‫رواﺑﻂ‬ ‫ﺑﺎ‬ ‫ﺷﺪه‬. ‫ﻣﺪل‬ ‫از‬ ‫اﮔﺮ‬‫ﻣﺨﺼـﻮص‬ ‫وزن‬ ‫ﭘـﺎراﻣﺘﺮ‬ ‫ﮐـﻪ‬ ‫رﯾﺎﺿـﯽ‬ ‫ﻫﺎي‬ ‫ﻧﺘـﺎﯾﺞ‬ ،‫ﺷـﻮد‬ ‫اﺳـﺘﻔﺎده‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﺮاي‬ ‫دارﻧﺪ‬ ‫ﺑﻪ‬ ‫ﻣﺘﻔﺎوﺗﯽ‬‫ﻣﯽ‬ ‫دﺳﺖ‬‫آﯾﺪ‬.‫اراﺋـﻪ‬ ‫راﺑﻄﻪ‬ ‫اﮔﺮ‬‫در‬ ‫ﺷـﺪه‬ACI363 ‫ﺑﻪ‬‫ﺑﻪ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﻧﺘﺎﯾﺞ‬ ‫رود‬ ‫ﮐﺎر‬‫آزﻣﺎﯾﺶ‬ ‫از‬ ‫آﻣﺪه‬ ‫دﺳﺖ‬ ‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬‫ﻃـﺮح‬ ‫ﻫﻤـﮥ‬ ‫در‬ ‫ﻟﯿﮑﺎ‬ ‫و‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬‫از‬ ‫ﻫـﺎ‬ ‫ﺑـﻪ‬ ‫ﻧﺘﺎﯾﺞ‬‫دﺳـﺖ‬‫ﮐﻮﭼـﮏ‬ ‫رﯾﺎﺿـﯽ‬ ‫ﻣـﺪل‬ ‫اﯾـﻦ‬ ‫از‬ ‫آﻣـﺪه‬‫و‬ ‫ﺗـﺮ‬ ‫ﺑﻮد‬ ‫ﺧﻮاﻫﺪ‬ ‫ﻏﯿﺮﻣﻨﻄﻘﯽ‬. ‫اراﺋﻪ‬ ‫راﺑﻄﻪ‬‫در‬ ‫ﺷﺪه‬BS8110‫ﺑﻪ‬ ‫را‬ ‫ﻧﺘﺎﯾﺠﯽ‬‫ﻣـﯽ‬ ‫دﺳﺖ‬‫دﻫـﺪ‬ ‫ﺗﺨﻤـ‬ ‫ﻧﺘـﺎﯾﺞ‬ ‫ﺑـﻮدن‬ ‫ﺑﯿﺸـﺘﺮ‬ ‫وﺟﻮد‬ ‫ﺑﺎ‬ ‫ﮐﻪ‬،‫واﻗﻌـﯽ‬ ‫ﻣﻘـﺎدﯾﺮ‬ ‫از‬ ‫ﯿﻦ‬ ‫اﺳﺖ‬ ‫ﮐﻢ‬ ‫اﺧﺘﻼف‬.‫ﻧﻤﻮﻧﻪ‬ ‫ﺑﺮاي‬ ‫ﺣﺘﯽ‬ ‫ﻧﺘﺎﯾﺞ‬‫ﻟﯿﮑـﺎ‬ ‫ﺣـﺎوي‬ ‫ﻫـﺎي‬ ‫ﻣﯽ‬ ‫ﻧﺰدﯾﮏ‬ ‫واﻗﻌﯿﺖ‬ ‫ﺑﻪ‬ ‫ﺑﯿﺸﺘﺮ‬‫ﺷﻮد‬.‫راﺑﻄﻪ‬‫ﻧﻮﯾﻞ‬‫ﻣﻘـﺎدﯾﺮي‬ ‫ﻧﯿـﺰ‬ ‫اراﺋﻪ‬ ‫راﺑﻄﻪ‬ ‫ﺣﺪ‬ ‫در‬‫در‬ ‫ﺷﺪه‬BS8110‫ﻣﯽ‬ ‫ﺗﺨﻤﯿﻦ‬‫راﺑﻄﻪ‬ ‫اﻣﺎ‬ ‫زﻧﺪ؛‬ ‫ﭘﺎﺋﯿﻦ‬ ‫ﺣﺪودي‬ ‫ﺗﺎ‬ ‫ﻣﻘﺎدﯾﺮي‬ ‫ﭘﻮﭘﻮوﯾﭻ‬‫رواﺑﻂ‬ ‫از‬ ‫ﺗﺮ‬‫اراﺋﻪ‬‫در‬ ‫ﺷـﺪه‬ BS8110‫ﻣﯽ‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﻧﻮﯾﻞ‬ ‫و‬‫زﻧﺪ‬.‫زده‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﻬﺘﺮﯾﻦ‬‫را‬ ‫ﺷـﺪه‬ ‫ﻣﯽ‬‫رواﺑـﻂ‬ ‫از‬ ‫ﻣﯿـﺎﻧﮕﯿﻦ‬ ‫ﮔـﺮﻓﺘﻦ‬ ‫ﺑﺎ‬ ‫ﺗﻮان‬‫اراﺋـﻪ‬‫ﺷـﺪه‬BS8110‫و‬ ‫ﺑﻪ‬ ‫ﭘﻮﭘﻮوﯾﭻ‬‫آورد‬ ‫دﺳﺖ‬. ‫ﺟﺪول‬)3(‫ﭘﻮآﺳﻮن‬ ‫ﺿﺮﯾﺐ‬ ،‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫آزﻣﺎﯾﺶ‬ ‫ﻧﺘﺎﯾﺞ‬ ‫ﺑﺘﻦ‬ ‫ﺑﺮﺷﯽ‬ ‫ﻣﺪول‬ ‫و‬ ‫ﻃﺮح‬ ‫ﻧﺎم‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬(GPa) ‫ﺿﺮﯾﺐ‬ ‫ﭘﻮاﺳﻮن‬ ‫ﻣﺪول‬‫ﺑﺮﺷﯽ‬ (GPa) L190/1419/026/6 L267/1518/064/6 L357/1819/080/7 S188/1620/070/5 S227/2122/044/7 S330/1922/089/6 ‫ﺟﺪول‬)4(‫راﯾﺞ‬ ‫از‬ ‫ﺑﺮﺧﯽ‬‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﺮاي‬ ‫رواﺑﻂ‬ ‫ﺗﺮﯾﻦ‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫آﺋﯿﻦ‬‫ﻧﺎﻣﻪ‬ ‫ﻣﺮﺑﻮط‬ ‫ﻣﺪول‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﺮاي‬ ‫ﻣﻌﻤﻮل‬ ‫رواﺑﻂ‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ACI-363R 0.5 s cE 3320f 6900  ‫ﻧﻮﯾﻞ‬-]23[0.5 1.5 s cE (3320f 6900)( ) 2320    BS-8110 ]24[2 0.33 6 s cuE 1.7 f 10    ‫ﭘﻮﭘﻮوﯾﭻ‬-]25[ 2 3 s cuE 1.19f ‫ﺟﺪول‬)5(‫ﺗﺨﻤﯿﻦ‬‫زده‬ ‫ﻫﺎي‬‫ﺑﻪ‬ ‫ﺷﺪه‬‫راﯾﺞ‬ ‫رواﺑﻂ‬ ‫وﺳﯿﻠﮥ‬(GPa) ‫ﭘﯿﺶ‬‫ﻣﻌﺘﺒﺮ‬ ‫رواﺑﻂ‬ ‫ﺑﺮاﺳﺎس‬ ‫ﺑﯿﻨﯽ‬(MPa) ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﺑﺪﺳﺖ‬‫آﻣﺪه‬ ‫ﻧﺎم‬ ‫ﻃﺮح‬ACI-363R ‫ﻧﻮﯾﻞ‬ BS-8110 ‫ﭘﻮﭘﻮوﯾﭻ‬ 25/25 26/16 88/15 17/13 90/14 L1 19/26 98/17 82/17 07/14 67/15 L2 47/27 06/20 11/20 32/15 57/18 L3 63/27 37/22 89/23 47/15 88/16 S1 90/28 03/24 65/25 73/16 27/21 S2 05/30 66/25 27/27 90/17 30/19 S3 ‫ﺳـﺒﮏ‬ ‫ﺧﺎص‬ ‫وﺿﻌﯿﺖ‬ ‫دﻟﯿﻞ‬ ‫ﺑﻪ‬ ‫اﺳﺖ‬ ‫ﻣﺴﻠﻢ‬‫ﻧـﻮع‬ ‫از‬ ‫داﻧـﻪ‬ ‫ﺑـﺮاي‬ ‫ﺧـﺎص‬ ‫ﻣـﺪل‬ ‫ﯾـﮏ‬ ‫اراﺋـﻪ‬ ‫ﺑـﻪ‬ ‫ﻧﯿـﺎز‬ ،‫اﯾﺮان‬ ‫ﺗﻮﻟﯿﺪ‬ ‫ﻟﯿﮑﺎي‬ ‫ﺑﺘﻦ‬‫ﻧﯿﻤﻪ‬ ‫ﻫﺎي‬‫ﺳﺒﮏ‬‫و‬ ‫ﭘﺮﻋﯿﺎر‬ ‫و‬ ‫ﮐﻢ‬ ‫ﺳﯿﻤﺎن‬ ‫ﺑﻪ‬ ‫آب‬ ‫ﻧﺴﺒﺖ‬ ‫ﺑﺎ‬ ‫داﻧﻪ‬ ‫ﻣﯽ‬ ‫اﺣﺴﺎس‬ ‫آن‬ ‫ﺑﺪون‬ ‫ﯾﺎ‬ ‫ﺳﯿﻠﯿﺴﯽ‬ ‫دوده‬ ‫داراي‬‫ﺷﻮد‬.
  • 7. ‫ﻋﻠﻤﯽ‬ ‫ﻣﺠﻠﻪ‬-‫ﻣﺪرس‬ ‫ﻋﻤﺮان‬ ‫ﭘﮋوﻫﺸﯽ‬‫ﺷﻤﺎره‬ ،‫دوازدﻫﻢ‬ ‫دوره‬4/‫زﻣﺴﺘﺎن‬1391 85 ‫ﺿﺮﯾﺐ‬ ‫ﺑﺮاي‬‫ﻣﯽ‬ ‫ﭘﯿﺸﻨﻬﺎد‬ ‫ﭘﻮاﺳﻮن‬‫ﻣﻘﺪار‬ ‫ﺷﻮد‬18/0‫ﺑـﺮاي‬ ‫ﺑﺘﻦ‬‫و‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬22/0‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬‫اﺳـﮑﻮرﯾﺎ‬ ‫ﺣـﺎوي‬ ‫ﻫﺎي‬ ‫ﺷﻮد‬ ‫ﻣﻨﻈﻮر‬. ‫ﻣـﺪول‬ ‫ﻣﻘﺪار‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬ ‫ﺑﺎ‬ ‫ﺑﺘﻮان‬ ‫ﮐﻪ‬ ‫اﯾﻦ‬ ‫ﺑﺮاي‬ ‫ﺳﺎده‬ ‫را‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬‫ﻣـﺪل‬ ً‫ﻻ‬‫ﻣﻌﻤﻮ‬ ‫آورد‬ ‫ﺑﺪﺳﺖ‬ ‫ﺗﺮ‬‫ﻫـﺎﯾﯽ‬ ‫ﻣﯽ‬ ‫اراﺋﻪ‬‫ﺷﻮد‬.‫ﻣﺪل‬‫ﺳﺎده‬ ‫رﯾﺎﺿﯽ‬ ‫ﻫﺎي‬‫ﻣﻮ‬ ‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬‫ﺟﻮد‬: Es= 0.478 fc + 0.13 (R=0.95) )5( Es= 0.255 fc + 7.942 (R=0.31) )6( Es= 1.15×1.19×fc 0.66 (R=0.98) )7( ‫رواﺑﻂ‬5،6‫و‬ ‫اﺳﮑﻮرﯾﺎ‬ ،‫ﻟﯿﮑﺎ‬ ‫ﺑﻪ‬ ‫ﻣﺮﺑﻮط‬ ‫ﺗﺮﺗﯿﺐ‬ ‫ﺑﻪ‬7‫ﺑﻪ‬ ‫ﻣﺮﺑﻮط‬ ‫اﺳﺖ‬ ‫دو‬ ‫ﻫﺮ‬.‫راﺑﻄـﻪ‬7‫اﻓﺰاﯾﻨـﺪه‬ ‫ﺿـﺮﯾﺐ‬15/1‫راﺑﻄـﻪ‬ ‫در‬ ‫را‬ ‫اﺳـﺖ‬ ‫ﮐﺮده‬ ‫اﻋﻤﺎل‬ ‫ﭘﻮﭘﻮوﯾﭻ‬.‫ﻣـﺪل‬ ‫ﺳـﻪ‬‫اراﺋـﻪ‬‫ﺿـﺮﯾﺐ‬ ‫ﺷـﺪه‬ ‫ـﺪ‬‫ـ‬‫ﻧﺪارﻧ‬ ‫ـﺎﻧﯽ‬‫ـ‬‫ﯾﮑﺴ‬ ‫ـﺘﮕﯽ‬‫ـ‬‫ﻫﻤﺒﺴ‬.‫ـﻪ‬‫ـ‬‫راﺑﻄ‬ ‫ـﺖ‬‫ـ‬‫ﺣﻘﯿﻘ‬ ‫در‬7‫ـﺮﯾﻦ‬‫ـ‬‫ﺑﻬﺘ‬ ‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬ ‫را‬ ‫ﺗﺨﻤﯿﻦ‬‫اﺳﺖ‬ ‫داده‬ ‫اراﺋﻪ‬ ‫ﻣﻮﺟﻮد‬ ‫ﻫﺎي‬. 3-3-‫ﻣﻨﺤﻨﯽ‬‫ﺗﻨﺶ‬ ‫ﻫﺎي‬-‫ﮐﺮﻧﺶ‬ ‫ﮔﻔﺘﻪ‬ ‫رواﺑﻂ‬ ‫از‬ ‫اﺳﺘﻔﺎده‬ ‫ﺑﺎ‬‫ﻣﻨﺤﻨـﯽ‬ ‫ﻣﻘﺪﻣـﻪ‬ ‫ﺑﺨﺶ‬ ‫در‬ ‫ﺷﺪه‬‫ﻫـﺎي‬ ‫ﺗﻨﺶ‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫ﻧﺰدﯾﮏ‬ ‫ﮐﻪ‬ ‫ﺷﺪ‬ ‫زده‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﻫﺎ‬‫ﺗﺨﻤـﯿﻦ‬ ‫ﺗﺮﯾﻦ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺑﻪ‬‫در‬ ‫واﻗﻌـﯽ‬ ‫ﻫﺎي‬‫ﺷـﮑﻞ‬‫ﻫـﺎي‬)1(‫و‬)2(‫ﺷـﺪه‬ ‫آورده‬ ‫اﺳﺖ‬.‫ﻧﺰدﯾﮏ‬ ‫ﺣﺘﯽ‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫ﻣﺸﺨﺺ‬ ‫ﮐﺎﻣﻼ‬‫ﺗﺨﻤـﯿﻦ‬ ‫ﺗﺮﯾﻦ‬‫ﻫـﺎ‬ ‫ﭼﺸـﻢ‬ ‫اﺧـﺘﻼف‬ ‫واﻗﻌﯽ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺑﺎ‬ ‫ﻧﯿﺰ‬‫ﻋـﻼوه‬ ‫ﺑـﻪ‬ ‫دارد؛‬ ‫ﮔﯿـﺮي‬ ‫ﻣﻨﺤﻨﯽ‬‫اﺳـﺖ‬ ‫ﻧﺰدﯾـﮏ‬ ‫ﺧﯿﻠﯽ‬ ‫ﺧﻄﯽ‬ ‫ﺣﺎﻟﺖ‬ ‫ﺑﻪ‬ ‫واﻗﻌﯽ‬ ‫ﻫﺎي‬.‫ﺑـﺎ‬ ‫ﺗـﻨﺶ‬ ‫راﺑﻄـﻪ‬ ‫ﻋﻤـﻮﻣﯽ‬ ‫روﻧﺪ‬ ‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬-‫ﺑـﺘﻦ‬ ‫در‬ ‫ﮐـﺮﻧﺶ‬‫ﻫـﺎي‬ ‫ﻧﯿﻤﻪ‬‫ﺳﺒﮏ‬‫ﺗﻤﺎم‬ ‫و‬ ‫داﻧﻪ‬‫ﺳﺒﮏ‬‫ﺧﻄـﯽ‬ ‫و‬ ‫داﻧـﻪ‬‫ﺑـﻮد‬‫ﺑﺨـﺶ‬ ‫در‬ ‫آن‬ ‫ن‬ ‫ﻋﻤﺪه‬‫ﻣﯽ‬ ‫ﻧﻈﺮ‬ ‫ﺑﻪ‬ ‫ﺻﻌﻮدي‬ ‫ﺷﺎﺧﻪ‬ ‫از‬ ‫اي‬‫ﮐـﺮد‬ ‫ﻗﺒـﻮل‬ ‫ﺑﺘﻮان‬ ‫رﺳﺪ‬ ‫رﻓﺘـﺎر‬ ‫و‬ ‫اﻻﺳﺘﯿﺴـﯿﺘﻪ‬ ‫ﻣـﺪول‬ ‫ﻧﺰدﯾﮑﯽ‬ ‫ﺧﺎﻃﺮ‬ ‫ﺑﻪ‬ ‫ﺣﺎﻟﺖ‬ ‫اﯾﻦ‬ ‫ﮐﻪ‬ ‫ﺳﺒﮏ‬ ‫و‬ ‫ﺳﯿﻤﺎن‬ ‫ﺧﻤﯿﺮ‬‫ﺑﻪ‬ ‫ﻟﯿﮑﺎ‬ ‫داﻧﻪ‬‫اﺳﺖ‬ ‫آﻣﺪه‬ ‫وﺟﻮد‬.‫ﺑـﺎ‬ ‫ﺷـﺎﯾﺪ‬ ‫ﺣﺪ‬ ‫ﺑﺘﻮان‬ ‫ﺣﺎﻟﺖ‬ ‫اﯾﻦ‬ ‫وﺟﻮد‬35‫ﯾﺎ‬40‫ﻓﺸـﺎري‬ ‫ﺗـﻨﺶ‬ ‫درﺻـﺪ‬ ‫ﺑ‬ ‫وﺗﺮي‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﺗﻌﯿﯿﻦ‬ ‫ﺑﺮاي‬ ‫ﮐﻪ‬ ‫ﻧﻬﺎﯾﯽ‬‫ﻪ‬‫ﻣـﯽ‬ ‫ﮐـﺎر‬‫رود‬ ‫ﺑﻪ‬ ‫را‬75‫ﯾﺎ‬80‫رﺳﺎﻧﺪ‬ ‫درﺻﺪ‬. 3-3-1-‫ﻣﺪل‬‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫رﯾﺎﺿﯽ‬ ‫ﻫﺎي‬-‫ﮐﺮﻧﺶ‬ ‫اﻟﻒ‬(‫ﺻﻌﻮدي‬ ‫ﺷﺎﺧﻪ‬ ‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬ ‫ﺑﺎ‬‫ﺷﮑﻞ‬)3(‫ﻣﯽ‬ ‫ﻧﻈﺮ‬ ‫ﺑﻪ‬‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﻬﺘﺮﯾﻦ‬ ‫رﺳﺪ‬‫ﺑـﺮاي‬ ‫ﻫﺎ‬ ‫ﺑﺘﻦ‬ ‫ﻣﺸﺨﺼﻪ‬ ‫ﻣﻨﺤﻨﯽ‬‫آزﻣﺎﯾﺶ‬ ‫ﻫﺎي‬‫ﻣـﺪول‬ ‫ﻣﺒﻨـﺎي‬ ‫ﺑـﺮ‬ ‫را‬ ‫ﺷـﺪه‬ ‫ﺑﺘﻦ‬ ‫ﺳﮑﺎﻧﺖ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬‫ﻣﯽ‬ ‫ﻫﺎ‬‫ﺑﺘﻦ‬ ‫اﯾﻦ‬ ‫رﻓﺘﺎر‬ ‫و‬ ‫زد‬ ‫ﺗﻮان‬‫ﺑـﺮ‬ ‫ﻫـﺎ‬ ‫ﺧﻼ‬‫ﺑﺘﻦ‬ ‫ف‬‫ﻣﻨﺤﻨـﯽ‬ ‫ﻧـﻮﻋﯽ‬ ‫از‬ ً‫ﻻ‬‫ﻣﻌﻤـﻮ‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫ﻣﻌﻤﻮﻟﯽ‬ ‫ﻫﺎي‬ ‫ﻣﯽ‬ ‫ﺗﺒﻌﯿﺖ‬ ‫دوم‬ ‫درﺟﻪ‬‫ﮐﻨﻨﺪ‬. ‫ﺷﮑﻞ‬)1(‫ﻣﻨﺤﻨﯽ‬‫ﺗﻨﺶ‬ ‫ﻫﺎي‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬(L1) ‫ﺷﮑﻞ‬)2(‫ﻣﻨﺤﻨﯽ‬‫ﺗﻨﺶ‬ ‫ﻫﺎي‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬(S1) ‫ﻣـﺪول‬ ‫ﺑـﻪ‬ ‫ﺷـﺪه‬ ‫زده‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﯾﮏ‬ ‫درﺟﻪ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺷﯿﺐ‬ ‫ﻧﺴﺒﺖ‬ ‫زﯾﺮ‬ ‫در‬ ‫ﺑﺘﻦ‬ ‫ﻫﺮ‬ ‫در‬ ‫ﺳﮑﺎﻧﺖ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬‫اﺳﺖ‬ ‫آﻣﺪه‬. ٠ ۵ ١٠ ١۵ ٢٠ ٢۵ ٣٠ ٣۵ ٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ‫(ﺗﻨﺶ‬MPa) ‫ﮐﺮﻧﺶ‬ L1 TODESCHINI ٠ ١٠ ٢٠ ٣٠ ۴٠ ۵٠ ٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ (‫ﺗﻨﺶ‬MPa) ‫ﮐﺮﻧﺶ‬ S1 HOGNESTAD
  • 8. ‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫و‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﺮرﺳﯽ‬-‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫داﻧﻪ‬‫ﭼﺎﻟﻪ‬ ‫ﻋﻠﯿﺮﺿﺎ‬ ‫و‬ ‫ﺧﺎﻧﺰادي‬ ‫ﻣﺼﻄﻔﯽ‬‫ﮐﺎﯾﯽ‬ 86 ‫ﺟﺪول‬)6(‫ﺗﺨﻤﯿﻦ‬ ‫ﯾﮏ‬ ‫درﺟﻪ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺷﯿﺐ‬‫زده‬‫ﺳﮑﺎﻧﺖ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﺑﻪ‬ ‫ﺷﺪه‬ ‫ﻃﺮح‬ ‫ﻧﻮع‬‫ﺷﯿﺐ‬ ‫ﻧﺴﺒﺖ‬‫ﻣﺪول‬ ‫ﺑﻪ‬ ‫ﻣﻨﺤﻨﯽ‬ L1120/1 L2058/1 L3977/0 S1977/0 S1936/0 S1950/0 ‫ﻣﺸﺎﻫﺪه‬ ‫ﺿﺮاﯾﺐ‬ ‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬ ‫ﺑﺎ‬‫ﺟﺪول‬ ‫در‬ ‫ﺷﺪه‬)6(‫ﻟﯿﮑـﺎ‬ ‫ﺑـﺮاي‬ ‫ﻧﺴـﺒﺖ‬ ‫ﻣﻨﺤﻨـﯽ‬ ‫ﺷـﯿﺐ‬ ،‫ﺑـﺘﻦ‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫اﻓﺰاﯾﺶ‬ ‫ﺑﺎ‬‫ﻣـﺪول‬ ‫ﺑـﻪ‬ ‫ﻣﯽ‬ ‫ﮐﺎﻫﺶ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬‫ﯾﺎﺑﺪ‬.‫ﺳـﻪ‬ ‫ﻫﺮ‬ ‫در‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺑﺎ‬ ‫راﺑﻄﻪ‬ ‫در‬ ‫ﺑـﻪ‬ ‫ﮐـﻪ‬ ‫اﺳـﺖ‬ ‫ﻣـﺪول‬ ‫از‬ ‫ﮐﻤﺘـﺮ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺷﯿﺐ‬ ،‫اﺧﺘﻼط‬ ‫ﻃﺮح‬ ‫داﻧـﻪ‬ ‫اﻻﺳﺘﯿﺴـﯿﺘﻪ‬ ‫ﻣـﺪول‬ ‫ﺑﻮدن‬ ‫ﺑﯿﺸﺘﺮ‬ ‫ﺧﺎﻃﺮ‬‫اﺳـﮑﻮرﯾﺎ‬ ‫ﻫـﺎي‬ ‫اﺳﺖ‬ ‫ﻟﯿﮑﺎ‬ ‫ﺑﻪ‬ ‫ﻧﺴﺒﺖ‬. ‫ﺷﮑﻞ‬)3(‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﺻﻌﻮدي‬ ‫ﻗﺴﻤﺖ‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫ﺳﺒﮏ‬ ‫ﻫﺎي‬‫داﻧﻪ‬ y = 16684x - 0.595 R² = 0.997 ٠ ١٠ ٢٠ ٣٠ ۴٠ ٠ ٠.٠٠٠۵ ٠.٠٠١ ٠.٠٠١۵ ٠.٠٠٢ L1 L1 Linear (L1) y = 16487x + 1.623 R² = 0.997 ٠ ١٠ ٢٠ ٣٠ ۴٠ ۵٠ ٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ S1 S1 Linear (S1) y = 16581x + 0.150 R² = 0.999 ٠ ١٠ ٢٠ ٣٠ ۴٠ ٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ L2 L2 Linear (L2) y = 19896x + 0.818 R² = 0.999 ٠ ١٠ ٢٠ ٣٠ ۴٠ ۵٠ ٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ S2 S2 Linear (S2) y = 18135x + 0.718 R² = 0.997 ٠ ١٠ ٢٠ ٣٠ ۴٠ ۵٠ ٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ L3 L٣ Linear (L ٣( y = 18347x + 1.002 R² = 0.997 ٠ ١٠ ٢٠ ٣٠ ۴٠ ۵٠ ۶٠ ٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ S3 S3 Linear (S3) Linear (S3)
  • 9. ‫ﻋﻠﻤﯽ‬ ‫ﻣﺠﻠﻪ‬-‫ﻣﺪرس‬ ‫ﻋﻤﺮان‬ ‫ﭘﮋوﻫﺸﯽ‬‫ﺷﻤﺎره‬ ،‫دوازدﻫﻢ‬ ‫دوره‬4/‫زﻣﺴﺘﺎن‬1391 87 ‫ب‬(‫ﻧﺰوﻟﯽ‬ ‫ﺷﺎﺧﻪ‬ ‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬ ‫ﺑﺎ‬‫ﺷﮑﻞ‬)4(‫ﻣـﯽ‬ ‫ﺗﻈـﺮ‬ ‫ﺑﻪ‬‫ﻣﺸﺨﺼـﯽ‬ ‫راﺑﻄـﻪ‬ ‫رﺳـﺪ‬ ‫ﻧﻤﯽ‬‫ﺑﺠـﺰ‬ ‫اﻣـﺎ‬ ‫داد؛‬ ‫ﭘﯿﺸـﻨﻬﺎد‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﻧﺰوﻟﯽ‬ ‫ﺷﺎﺧﻪ‬ ‫ﺑﺮاي‬ ‫ﺗﻮان‬ ‫ﺑﺘﻦ‬L1‫ﻣﻨﺤﻨـﯽ‬ ‫ﺷـﮑﻞ‬ ‫ﺑـﻪ‬ ‫ﺗﻘﺮﯾـﺐ‬ ‫ﺑـﺎ‬ ‫آن‬ ‫ﻧﺰوﻟﯽ‬ ‫ﺷﺎﺧﻪ‬ ‫ﮐﻪ‬ ،‫دارد‬ ‫ﺧﻄـﯽ‬ ‫ﻣﻨﺤﻨـﯽ‬ ‫ﺑـﻪ‬ ‫ﻧﺴﺒﺖ‬ ‫ﺑﻬﺘﺮي‬ ‫ﻫﻤﺒﺴﺘﮕﯽ‬ ‫دو‬ ‫درﺟﻪ‬ ‫ﺑﺘﻦ‬ ‫ﺑﺎﻗﯽ‬‫ﺷـ‬ ‫ﺑـﺎ‬ ‫ﻫـﺎ‬‫و‬ ‫ﺻـﻌﻮدي‬ ‫ﺷـﺎﺧﻪ‬ ‫از‬ ‫ﮐﻤﺘـﺮ‬ ‫ﻣﻨﻔـﯽ‬ ‫ﯿﺐ‬ ‫ﺑﻪ‬‫اﺳـﺖ‬ ‫ﺧﻄـﯽ‬ ‫ﺻﻮرت‬.‫ﺗـﻨﺶ‬ ‫ﺑﯿﺸـﯿﻨﻪ‬ ‫ﺑـﺎ‬ ‫ﻣﺘﻨـﺎﻇﺮ‬ ‫ﮐـﺮﻧﺶ‬ ‫ﺛﺒﺖ‬‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬ ‫ﻣﻨﺤﻨﯽ‬ ‫در‬ ‫ﺷﺪه‬‫ﺣﺪود‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬2000 ‫ﺑﺘﻦ‬ ‫ﺑﺮاي‬ ‫و‬ ‫ﻣﯿﮑﺮوﮐﺮﻧﺶ‬‫ﺣﺪود‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬2500 ‫اﺳﺖ‬ ‫ﺑﻮده‬ ‫ﻣﯿﮑﺮوﮐﺮﻧﺶ‬. ‫ﺷﮑﻞ‬)4(‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫ﻧﺰوﻟﯽ‬ ‫ﻗﺴﻤﺖ‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫ﺳﺒﮏ‬ ‫ﻫﺎي‬‫داﻧﻪ‬ y = -8518x + 48.43 R² = 0.982 y = -2E+06x2 + 4415.x + 31.52 R² = 0.996 ٠ ۵ ١٠ ١۵ ٢٠ ٢۵ ٣٠ ٣۵ ٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ٠.٠٠۴ L1 L1 Linear (L1) Poly. (L1) y = -13861x + 72.95 R² = 0.999 ٠ ١٠ ٢٠ ٣٠ ۴٠ ۵٠ ٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ٠.٠٠۴ S1 S١ Linear (S١( y = -11865x + 59.55 R² = 0.995 ٠ ١٠ ٢٠ ٣٠ ۴٠ ٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ٠.٠٠۴ L2 L2 Linear (L2) y = -16438x + 83.67 R² = 0.998 ٠ ١٠ ٢٠ ٣٠ ۴٠ ۵٠ ٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ٠.٠٠۴ S2 S2 Linear (S2) y = -13762x + 72.62 R² = 0.998 ٠ ١٠ ٢٠ ٣٠ ۴٠ ۵٠ ٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ٠.٠٠۴ L3 L3 Linear (L3) y = -14880x + 90.11 R² = 0.996 ٠ ١٠ ٢٠ ٣٠ ۴٠ ۵٠ ۶٠ ٠.٠٠١ ٠.٠٠٢ ٠.٠٠٣ ٠.٠٠۴ S3 Series1 Linear (S3)
  • 10. ‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫و‬ ‫ﻣﮑﺎﻧﯿﮑﯽ‬ ‫ﻣﺸﺨﺼﺎت‬ ‫ﺑﺮرﺳﯽ‬-‫ﺳﺒﮏ‬ ‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫داﻧﻪ‬‫ﭼﺎﻟﻪ‬ ‫ﻋﻠﯿﺮﺿﺎ‬ ‫و‬ ‫ﺧﺎﻧﺰادي‬ ‫ﻣﺼﻄﻔﯽ‬‫ﮐﺎﯾﯽ‬ 88 4-‫ﻧﺘﯿﺠﻪ‬‫ﮔﯿﺮي‬ ‫ﺑﺮرﺳﯽ‬ ‫ﺑﻪ‬ ‫ﺗﻮﺟﻪ‬ ‫ﺑﺎ‬‫ﺗﺤﻠﯿﻞ‬ ‫و‬ ‫ﺗﺠﺰﯾﻪ‬ ‫و‬ ‫آزﻣﺎﯾﺸﮕﺎﻫﯽ‬ ‫ﻫﺎي‬‫ﻫـﺎي‬ ‫اﻧﺠﺎم‬‫ﻣﯽ‬ ‫ﺷﺪه‬‫ﻧﺘﯿﺠﻪ‬ ‫ﺗﻮان‬‫ﮔﯿﺮي‬‫ﻧﻤﻮد‬ ‫ﻣﻄﺮح‬ ‫را‬ ‫زﯾﺮ‬ ‫ﻧﻬﺎﯾﯽ‬ ‫ﻫﺎي‬: 1.‫ﻋﯿـﺎر‬ ‫ﺑـﺎ‬ ‫ﺳﯿﻤﺎﻧﯽ‬ ‫ﻣﻮاد‬ ‫از‬ ‫اﺳﺘﻔﺎده‬ ‫ﺑﺎ‬Kg/m3 500‫ﻧﺴـﺒﺖ‬ ‫و‬ ‫ﺳﯿﻤﺎن‬ ‫ﺑﻪ‬ ‫آب‬30/0‫ﻣﯿـﺰان‬ ‫ﺑـﻪ‬ ‫ﺳﯿﻠﯿﺴﯽ‬ ‫دوده‬ ‫ﺟﺎﯾﮕﺰﯾﻨﯽ‬ ،10 ‫اﻧـﺪازه‬ ‫ﺑﯿﺸـﯿﻨﮥ‬ ‫ﺑـﺎ‬ ‫ﻟﯿﮑﺎ‬ ،‫ﺳﯿﻤﺎن‬ ‫وزن‬ ‫درﺻﺪ‬5/12‫ﻣﺘـﺮ‬ ‫ﻣﯿﻠـﯽ‬ )10-3(‫ﻧﻮع‬ ‫ﭘﺮﺗﻠﻨﺪ‬ ‫ﺳﯿﻤﺎن‬ ،‫ﻣﻌﻤﻮﻟﯽ‬ ‫ﻣﺎﺳﻪ‬ ،1‫ﻓﻮق‬ ،‫روان‬‫ﮐﻨﻨﺪه‬ ‫ﻣﯿﺰان‬ ‫ﺑﻪ‬1‫ﻣﻘﺎوﻣـﺖ‬ ‫ﺑﯿﺸـﺘﺮﯾﻦ‬ ،‫ﺳـﯿﻤﺎﻧﯽ‬ ‫ﻣـﻮاد‬ ‫وزن‬ ‫درﺻـﺪ‬ ‫ﻓﺸﺎري‬28‫ﺑﺘﻦ‬ ‫ﺑﯿﻦ‬ ‫روزه‬‫ﺳﺒﮏ‬ ‫ﻫﺎي‬‫ﻣﺮ‬ ،‫داﻧﻪ‬‫ﻣﺨﻠـﻮط‬ ‫ﺑـﻪ‬ ‫ﺑﻮط‬ S3‫ﺑﺮاﺑـﺮ‬ ‫ﻣﮑﻌﺒـﯽ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫ﺑﺮاي‬ ‫ﮐﻪ‬ ‫ﺑﻮده‬MPa63/54‫ﺑـﺮاي‬ ‫و‬ ‫اﺳﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬‫ﺑﺮاﺑﺮ‬ ‫اي‬MPa62/48‫اﺳـﺖ‬.‫ﻣﻘﺎوﻣـﺖ‬ ‫ﮐﻤﺘـﺮﯾﻦ‬ ‫ﻓﺸﺎري‬28‫ﻣﺨﻠﻮط‬ ‫ﺑﻪ‬ ‫ﻣﺮﺑﻮط‬ ‫روزه‬L1‫ﻧﻤﻮﻧـﻪ‬ ‫ﺑﺮاي‬ ‫ﮐﻪ‬ ‫اﺳﺖ‬ ‫ﺑﺮاﺑﺮ‬ ‫ﻣﮑﻌﺒﯽ‬MPa2/33‫اﺳـﺘﻮاﻧﻪ‬ ‫ﻧﻤﻮﻧﻪ‬ ‫ﺑﺮاي‬ ‫و‬‫ﺑﺮاﺑـﺮ‬ ‫اي‬MPa 54/30‫اﺳﺖ‬.‫ﺑﺘﻦ‬ ‫وزن‬ ‫ﮐﺎﻫﺶ‬‫ﻟﯿﮑـﺎ‬ ‫ﺣـﺎوي‬ ‫ﻫﺎي‬‫ﺣـﺪود‬30 ‫ﺑﺘﻦ‬ ‫و‬ ‫درﺻﺪ‬‫ﺣـﺪود‬ ‫اﺳـﮑﻮرﯾﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬20‫ﺑـﻮد‬ ‫درﺻـﺪ‬. ‫ﻣﻘﺎوﻣﺖ‬ ‫ﻧﺘﺎﯾﺞ‬‫ﻓﺸﺎري‬ ‫ﻫﺎي‬28‫آزﻣﻮﻧﻪ‬ ‫وزن‬ ‫ﺗﺎﺑﻊ‬ ً‫ﻼ‬‫ﻋﻤ‬ ‫روزه‬‫ﻫﺎ‬ ‫ﻣﯽ‬ ‫ﮐﺎﻫﺶ‬ ‫ﻧﯿﺰ‬ ‫ﻣﻘﺎوﻣﺖ‬ ،‫آن‬ ‫ﮐﺎﻫﺶ‬ ‫ﺑﺎ‬ ‫و‬ ‫اﺳﺖ‬‫ﯾﺎﺑﺪ‬. 2.‫ﺑﺘﻦ‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬ ‫اﻻﺳﺘﯿﺴﯿﺘﻪ‬ ‫ﻣﺪول‬‫ﺗﻮﺟـﻪ‬ ‫ﺑﺎ‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬ ‫داﻧﻪ‬ ‫ﺑﺎﻓﺖ‬ ‫ﺑﻪ‬‫ﺣﺪود‬ ‫ﺑﯿﻦ‬ ‫ﺑﻨﺪي‬15‫ﺗﺎ‬19‫ﺑﻮد‬ ‫ﮔﯿﮕﺎﭘﺎﺳﮑﺎل‬.‫اﯾﻦ‬ ‫ﺑـﺘﻦ‬ ‫ﺑﺮاي‬ ‫ﻣﻘﺪار‬‫ﺑـﯿﻦ‬ ‫اﺳـﮑﻮرﯾﺎ‬ ‫ﺣـﺎوي‬ ‫ﻫـﺎي‬17‫ﺗـﺎ‬50/19 ‫ﺑﻮد‬ ‫ﮔﯿﮕﺎﭘﺎﺳﮑﺎل‬.‫اﻻﺳﺘﯿﺴـﯿﺘﻪ‬ ‫ﻣﺪول‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﺮاي‬ ‫ﻧﯿﺰ‬ ‫رواﺑﻄﯽ‬ ‫ﺑـﺘﻦ‬ ‫اﯾﻦ‬ ‫اﺳﺘﺎﺗﯿﮑﯽ‬‫وزن‬ ‫و‬ ‫ﻓﺸـﺎري‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫اﺳـﺎس‬ ‫ﺑـﺮ‬ ‫ﻫـﺎ‬ ‫اﺳﺖ‬ ‫ﺷﺪه‬ ‫اراﺋﻪ‬ ‫ﻣﺨﺼﻮﺻﺸﺎن‬. 3.‫ﭘﻮاﺳﻮن‬ ‫ﺿﺮاﯾﺐ‬‫ﺑﺘﻦ‬‫ﻃـﻮر‬ ‫ﺑﻪ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬ ‫ﻣﺘﻮﺳﻂ‬19/0‫و‬22/0‫ﺷﺪ‬ ‫ﺗﻌﯿﯿﻦ‬. 4.‫ﻧﺴ‬‫ﻧﻤﻮﻧﻪ‬ ‫ﻓﺸﺎري‬ ‫ﻣﻘﺎوﻣﺖ‬ ‫ﺒﺖ‬‫اﺳـﺘﻮاﻧﻪ‬ ‫ﺑـﻪ‬ ‫ﻣﮑﻌﺒﯽ‬ ‫ﻫﺎي‬‫اي‬ ‫ﺑﺘﻦ‬ ‫در‬‫از‬ ‫ﮐﻤﺘﺮ‬ ‫اﺳﮑﻮرﯾﺎ‬ ‫و‬ ‫ﻟﯿﮑﺎ‬ ‫ﺣﺎوي‬ ‫ﻫﺎي‬1‫ﻣﺤـﺪوده‬ ‫در‬ ‫و‬ 92/0‫ﺗﺎ‬89/0‫ﺷﺪ‬ ‫ﺛﺒﺖ‬. 5.‫ﺗﻨﺶ‬ ‫ﻣﻨﺤﻨﯽ‬-‫ﺑﺘﻦ‬ ‫ﮐﺮﻧﺶ‬‫ﻣﻄﺎﻟﻌﻪ‬ ‫ﻫﺎي‬‫ﺷـﺎﺧﻪ‬ ‫در‬ ‫ﺷﺪه‬‫ﻫـﺎي‬ ‫اﺳﺖ‬ ‫ﺑﻮده‬ ‫ﻣﻨﻔﯽ‬ ً‫ﺎ‬‫ﺗﻘﺮﯾﺒ‬ ،‫ﻧﺰوﻟﯽ‬ ‫و‬ ‫ﺻﻌﻮدي‬.‫ﺗﻮﺻـﯿﻪ‬‫ﻧﯿـﺰ‬ ‫ﻫـﺎﯾﯽ‬ ‫ﻣﻨﺤﻨﯽ‬ ‫اﯾﻦ‬ ‫ﺗﺨﻤﯿﻦ‬ ‫ﺑﺮاي‬‫ﺷﺪ‬ ‫اراﺋﻪ‬ ‫ﻫﺎ‬. 5-‫ﻣﺮاﺟﻊ‬ [1] Topcu I.B., "Semi-lightweight concretes produced by volcanic slags", Cem Concr Res 27(1) (1997) 15-21 [2] Al-Khaiat H., Haque M.N., "Effect of initial curing on early strength and physical properties of lightweight concrete", Cem Concr Res 28(6) (1998) 859-866 [3] Ke Y., Beacour A.L., Ortola S., Dumontets H., Cabrillac R., "Influence of volume fraction and characteristics of lightweight aggregates on the mechanical properties of concrete", Cons Build Mat 23 (2009) 2821-2828 ]4[،‫ﻣﺤﺴـﻦ‬ ،‫ﺗﺪﯾﻦ‬"‫و‬ ‫ﺑﺮرﺳـﯽ‬‫ارزﯾـﺎﺑﯽ‬،‫ﮐﺸﺸـﯽ‬ ‫ﻣﻘﺎوﻣـﺖ‬ ‫ﺑـﺘﻦ‬ ‫ﺧﻮردﮔﯽ‬ ‫ﺷﺪت‬ ‫و‬ ‫ﭘﻮاﺳﻮن‬ ‫ﺿﺮﯾﺐ‬ ،‫ارﺗﺠﺎﻋﯽ‬ ‫ﻣﺪول‬ ‫ﭘﺮ‬ ‫ﺳﺒﮏ‬‫اﯾﺮان‬ ‫در‬ ‫ﻣﻮﺟﻮد‬ ‫ﻣﺼﺎﻟﺢ‬ ‫ﺑﺎ‬ ‫ﻣﻘﺎوﻣﺖ‬"‫ﭘﺎﯾـﺎن‬ ،‫ﻧﺎﻣـﻪ‬ ،‫اﯾـﺮان‬ ‫ﺻـﻨﻌﺖ‬ ‫و‬ ‫ﻋﻠﻢ‬ ‫داﻧﺸﮕﺎه‬ ،‫ﻋﻤﺮان‬ ‫داﻧﺸﮑﺪه‬ ،‫دﮐﺘﺮي‬ ‫ﺷﻬﺮﯾﻮر‬1381. [5] Demirboga R., Orung I., Gul R., "Effects of expanded perlite aggregate and mineral admixtures on the compressive strength of low- density concretes". Cement Concrete Res. 31(11) (2001) 1627-1632 [6] Chen H.J., Yen T., Lia T.P., Huang Y.L., "Determination of dividing strength and it's relation to the concrete strength in lightweight aggregate concrete", Cement and Concrete Composition,Vol. 21, (1999) 29-37 [7] European Union-Brite Euram III, "Definitions and international consensus report, BE96- 3942/R1", 1998 [8] Zhang M.H., Gjorv O.E., "Characteristics of lightweight aggregates for high-strength concrete", ACI Mater. J., 1991(March-April) 150-158 [9] Yang C.C., Huang R., "Approximate strength of lightweight aggregate using micromechanics
  • 11. ‫ﻋﻠﻤﯽ‬ ‫ﻣﺠﻠﻪ‬-‫ﻣﺪرس‬ ‫ﻋﻤﺮان‬ ‫ﭘﮋوﻫﺸﯽ‬‫ﺷﻤﺎره‬ ،‫دوازدﻫﻢ‬ ‫دوره‬4/‫زﻣﺴﺘﺎن‬1391 89 method", Adv. Cem. Based Mater., 7(3-4) (1998) 133-138 [10] Wasserman R., Bentur A., "Effect of lightweight fly ash aggregate microstructure on the strength of concretes", Cem. Concr. Res., 27(4) (1997) 525-537 [11] Kilic A., Atis C.D., Yasar E., Ozcan F., "High- strength lightweight concrete made with scoria aggregate containing mineral admixtures", Cem Concr Res, 33 (2003) 1595-1599 [12] Macgregor J.G., "Reinforced concrete mechanics and design", Prentice Hall, 3rd Edition, 1997 [13] Hognestad E., "A study of combined bending and axial load in reinforced concrete members", Bulletin 399, University of Illinois Engineering Experiment Station, Urbana, I11., November 1951, 128 [14] Todeschini C.E., Bianchini A.C., and Clyde E. Kesler, "Behavior of concrete columns reinforced with high strength steels", ACI Journal, Proceedings. Vol. 61, No. 6, June 1964, 701-716 [15] Popovics S., "A numerical approach to the complete stress-strain curve of concrete", Cement and Concrete Research, Vol. 3, (1973) 583-599 [16] Yi S.T., Kim J.K., Oh T.K., "Effect of strength and age on the stress-strain curves of concrete specimens", Cement and Concrete Research, Vol. 33, (2003) 1235-1244 [17] Blechman I., "Stage model of stress-strain relationship for concrete under short-term load – Part.1", Cement and Concrete Research, Vol. 18, (1988) 863-873 [18] ASTM C330-99, "Standard specification for lightweight aggregates for structural concrete", American Society for Testing And Materials, March 1999 [19] ASTM C150-99a, "Standard specification for portland cement", American Society For Testing And Materials, November 1999 [20] ASTM C 494/C 494M – 99a, "Standard specification for chemical admixtures for concrete", American Society For Testing And Materials, December 1999 [21] ACI 211.2-98, "Standard practice for selecting proportions for structural lightweight concrete", American Concrete Institute, 1998 ]22[،‫ﻫﺮﻣﺰ‬ ،‫ﻓﺎﻣﯿﻠﯽ‬"‫ﺑﺘﻦ‬ ‫ﺧﻮاص‬"‫ﭼـﺎپ‬ ،‫ﺑﯿﺮوﻧﯽ‬ ‫اﺑﻮرﯾﺤﺎن‬ ، ،‫اول‬1378 [23] Neville A.M., "Properties of concrete", Longman, 3rd Edition, 1981 [24] Slate F.O., Nilson A.H., Martinez S., "Mechanical properties of high strength lightweight concrete", ACI Materials Journal, Vol.3, (1986) 606-613 [25] Popovics S., "Strength and related properties of concrete, a quantitative approach", JohnWiley, 1998